MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC XYLEX™ X7507 PC+Polyester (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/PET Polyester Blend

Material Notes: F-1 weathering certified in natural color, specially designed for Pool & Spa applications.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Density 1.20 g/cc0.0434 lb/in³ISO 1183
Water Absorption 0.32 %0.32 %23°C/sat; ISO 62
Moisture Absorption 0.120 %0.120 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0080 in/in
@Thickness 0.126 in
SABIC method
Melt Flow  5.0 g/10 min
@Load 2.16 kg,
Temperature 265 °C
5.0 g/10 min
@Load 4.76 lb,
Temperature 509 °F
cm³/10 min; ISO 1133
 8.0 g/10 min
@Load 2.16 kg,
Temperature 265 °C
8.0 g/10 min
@Load 4.76 lb,
Temperature 509 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 59.0 MPa8560 psi50 mm/min; ISO 527
 65.0 MPa9430 psi50 mm/min; ASTM D638
Tensile Strength, Yield 61.0 MPa8850 psi50 mm/min; ASTM D638
 62.0 MPa8990 psi50 mm/min; ISO 527
Elongation at Break 110 %110 %50 mm/min; ISO 527
 130 %130 %50 mm/min; ASTM D638
Elongation at Yield 5.4 %5.4 %50 mm/min; ISO 527
 6.0 %6.0 %50 mm/min; ASTM D638
Tensile Modulus 2.30 GPa334 ksi5 mm/min; ASTM D638
 2.66 GPa386 ksi1mm/min; ISO 527
Flexural Yield Strength 92.0 MPa13300 psi2 mm/min; ISO 178
 96.0 MPa13900 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.18 GPa316 ksi2 mm/min; ISO 178
 2.32 GPa336 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 9.90 J/cm18.5 ft-lb/inASTM D256
 2.00 J/cm
@Temperature -30.0 °C
3.75 ft-lb/in
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO) 9.00 kJ/m²4.28 ft-lb/in²80*10*4; ISO 180/1A
 6.00 kJ/m²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 2.00 J/cm²9.52 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 79.0 J58.3 ft-lbASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  63.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
35.0 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 105 °C221 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 104 °C
@Thickness 3.20 mm
219 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 125 °C257 °FRate B/50; ISO 306
 125 °C257 °FRate B/50; ASTM D1525
 127 °C261 °FRate B/120; ISO 306
 
Optical PropertiesMetricEnglishComments
Haze 1.6 %
@Thickness 2.54 mm
1.6 %
@Thickness 0.100 in
ASTM D1003
Transmission, Visible >= 85 %
@Thickness 2.54 mm
>= 85 %
@Thickness 0.100 in
ASTM D1003
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 250 - 270 °C482 - 518 °FInjection Molding
Zone 1 240 - 250 °C464 - 482 °F
Zone 2 245 - 265 °C473 - 509 °F
Zone 3 250 - 270 °C482 - 518 °F
Melt Temperature 250 - 270 °C482 - 518 °F
Mold Temperature 45.0 - 60.0 °C113 - 140 °F
Drying Temperature 80.0 - 95.0 °C176 - 203 °FInjection Molding
Dry Time 3.00 - 5.00 hour3.00 - 5.00 hourInjection Molding
 8.00 hour8.00 hourCumulative; Injection Molding
Moisture Content 0.020 %0.020 %
Back Pressure 0.200 - 0.500 MPa29.0 - 72.5 psi
Shot Size 40 - 80 %40 - 80 %
Vent Depth 0.00130 - 0.00200 cm0.000512 - 0.000787 in
Screw Speed 20 - 100 rpm20 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI11633 / 245100

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.