MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Mitsubishi Reny® 1022HS Polyamide
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: 50% glass fiber reinforced. General grade. High Performance Polyamide. Reny is a proprietary molding compound based on mainly polyamide MXD6 that has been reinforced with glass fiber, carbon fiber or special minerals. Reny generally has superior mechanical strength and modulus compared with other engineering plastics. Thus, Reny is suitable as a metal substitute in many applications, including automobiles, electronics, electrical appliances, machinery, and construction. Excellent mechanical strength and modulus over a wide range of temperatures. Superior to commodity polyamides in dimensional stability and mechanical strength due to low water absorption. Low thermal expansion coefficient, equivalent to that of metal alloys. Highly resistant to oils and organic solvents. Low mold shrinkage and low warpage. Good surface finish even in highly filled grades.

Information provided by Mitsubishi Engineering Plastics Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.66 g/ccISO 1183
Water Absorption 0.87 %
@Temperature 23.0 °C
Immersion
Moisture Absorption 0.100 %
@Temperature 23.0 °C
50% RH
Linear Mold Shrinkage 0.0034 cm/cm
Melt Flow 6.0 g/10 min
@Load 2.16 kg,
Temperature 275 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 233 MPa50% RH; ISO 527-1,2
 236 MPadry; ISO 527-1,2
Elongation at Break 1.5 %dry; ISO 527-1,2
 1.6 %50% RH; ISO 527-1,2
Tensile Modulus 21000 MPa50% RH; ISO 527-1,2
 21850 MPadry; ISO 527-1,2
Flexural Strength 326 MPa50% RH; ISO 178
 384 MPadry; ISO 178
Flexural Modulus 19000 MPa50% RH; ISO 178
 19100 MPadry; ISO 178
Charpy Impact Unnotched 40.0 kJ/m²50% RH; ISO 179-1, 179-2
 61.0 kJ/m²dry; ISO 179-1, 179-2
Charpy Impact, Notched 11.8 kJ/m²dry; ISO 179-1, 179-2
 12.0 kJ/m²50% RH; ISO 179-1, 179-2
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmdry; IEC 60093
Surface Resistance 5.00e+15 ohmdry; IEC 60093
Dielectric Constant 4.7
@Frequency 1e+6 Hz
dry; IEC 60250
Dielectric Strength 24.0 kV/mm
@Thickness 2.00 mm
dry; IEC 60243-1
 33.0 kV/mm
@Thickness 1.00 mm
dry; IEC 60243-1
Dissipation Factor 0.0090
@Frequency 1e+6 Hz
dry; IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 10.0 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 40.0 µm/m-°CISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 245 °Cdry; ISO 75-1,2
Flammability, UL94 HB
@Thickness 1.60 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 280 °C
Middle Barrel Temperature 275 °C
Front Barrel Temperature 270 °C
Nozzle Temperature 280 °C
Mold Temperature 120 - 140 °C
Injection Pressure 20.0 - 150 MPa
Screw Speed 60 - 150 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsubishi Reny® 1025 Polyamide
Mitsubishi Reny® 1035 Polyamide
Mitsubishi Reny® 1071 Polyamide
Mitsubishi Reny® 1527 Polyamide
Ensinger TECATOR™ GF30 (XP142T) Polyamide-imide (PAI), 30% glass filled, compression molded

PMITSU9019 / 191692

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.