MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics WDS® High Porextherm
Categories: Ceramic; Oxide; Silicon Oxide

Material Notes: Silicate. WDS® High is a microporous insulation material which has an extremely low thermal conductivity coefficient giving it very good insulating properties. WDS® High can be protected by various wrapping possibilities, this allows an easy and dust-free installation as well as protecting the product from moisture. WDS® High consists of inorganic silicates. The main constituent is fumed silica; the other components are opacifiers to minimize infrared radiation. WDS® High (core material) is not flammable and meets the requirements acc. to DIN EN 13501-1 for fire protection class A1.

Application: Tried and tested applications for WDS® High include insulation for heat-treatment furnaces in the aluminum industry and back-up insulation in the industrial furnace industry.

Information provided by Morgan Advanced Materials

Key Words: Porextherm
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.250 - 0.310 g/cc
 
Mechanical PropertiesOriginal ValueComments
Compressive Strength 1.30 MPa
@Temperature 600 °C
ASTM C 165
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 0.220 BTU/lb-°F
@Temperature 700.0 °C
DIN 51007
Thermal Conductivity <= 0.0220 W/m-K
@Temperature 50.0 °C
ASTM C 177
 0.0220 W/m-K
@Temperature 200 °C
ASTM C 177
 0.0300 W/m-K
@Temperature 400 °C
ASTM C 177
 0.0430 W/m-K
@Temperature 600 °C
ASTM C 177
 0.0600 W/m-K
@Temperature 800 °C
ASTM C 177
Shrinkage 0.60 %
@Treatment Temp. 1000 °C,
Time 43200 sec
exposed on single side AAW-906-00
 1.6 %
@Treatment Temp. 950 °C,
Time 86400 sec
full soak
 3.5 %
@Treatment Temp. 1000 °C,
Time 86400 sec
full soak
 
Descriptive Properties
Classification Temperature (°C)1100
Colorwhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium AM60A-F, Die Cast
Magnesium AZ80A-T5, Forged
JIS S45C Steel, Normalized
Aluminum 1100-O

CMORF6109 / 202893

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.