MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

ALM PA 650 Nylon 12 SLS Prototyping Polymer
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: Combines strength, durability (high impact) and chemical resistance and produces strong, durable, end use prototype parts. SL parts are less porous, more precise and have less noticeable build lines than FDM (Fused Deposition Modeling) parts. LS systems build in 0.004-0.006 inch layers.

Information provided by Axis Prototypes.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.


Axis Proto Inc. Innovative leaders in producing high quality Rapid Prototyping and Rapid Manufacturing solutions using all major 3D printing systems including Stereolithography technology. Free online quotes at www.axisproto.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Bulk Density 0.460 g/cc0.0166 lb/in³ASTM D1895
Density 1.02 g/cc0.0368 lb/in³Sintered Part; ASTM D792
Particle Size 55 µm55 µmAverage D50; Laser Diffraction
 30 - 100 µm30 - 100 µmRange (D10 to D90); Laser Diffraction
Melt Flow 50 g/10 min
@Load 5.00 kg,
Temperature 235 °C
50 g/10 min
@Load 11.0 lb,
Temperature 455 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 48.0 MPa6960 psiXY direction; ASTM D638
Elongation at Break 24 %24 %XY direction; ASTM D638
Tensile Modulus 1.70 GPa247 ksiXY direction; ASTM D638
Flexural Modulus 1.50 GPa218 ksiXY direction; ASTM D790
Izod Impact, Notched 2.20 J/cm4.12 ft-lb/inASTM D256
Izod Impact, Unnotched 4.40 J/cm8.24 ft-lb/inASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 3.10e+14 ohm-cm3.10e+14 ohm-cm50% RH; 500V; ASTM D257
Surface Resistance 3.00e+14 ohm3.00e+14 ohm50% RH; 500V; ASTM D257
Dielectric Constant 2.92.950% RH; 500V; ASTM D150
 
Thermal PropertiesMetricEnglishComments
Melting Point 181 °C358 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 177 °C351 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 86.0 °C187 °FASTM D648
 
Descriptive Properties
ColorWhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polycarbonate, Extruded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Extruded
Overview of materials for Nylon 12
ALM PA 250 Nylon 12 SLS Prototyping Polymer
Chi Mei Wonderloy® PC-510 PC/ABS Alloy - Flame Retardant

PALAP98 / 142933

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.