Physical Properties | Metric | English | Comments |
---|
Density | 7.90 g/cc | 0.285 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Vickers | 160 | 160 |
Tensile Strength, Ultimate | 710 MPa | 103000 psi |
| 58.0 MPa @Temperature 1000 °C | 8410 psi @Temperature 1830 °F |
| 95.0 MPa @Temperature 900 °C | 13800 psi @Temperature 1650 °F |
| 170 MPa @Temperature 800 °C | 24700 psi @Temperature 1470 °F |
Tensile Strength, Yield | 365 MPa @Strain 0.2 % | 52900 psi @Strain 0.2 % |
Elongation at Break | 30 % | 30 % |
Creep Strength | 4.00 MPa @Temperature 1000 °C, Time 3.60e+6 sec | 580 psi @Temperature 1830 °F, Time 1000 hour |
| 20.0 MPa @Temperature 800 °C, Time 3.60e+6 sec | 2900 psi @Temperature 1470 °F, Time 1000 hour |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000104 ohm-cm | 0.000104 ohm-cm |
| 0.000107 ohm-cm @Temperature 100 °C | 0.000107 ohm-cm @Temperature 212 °F |
| 0.000110 ohm-cm @Temperature 200 °C | 0.000110 ohm-cm @Temperature 392 °F |
| 0.000114 ohm-cm @Temperature 300 °C | 0.000114 ohm-cm @Temperature 572 °F |
| 0.000116 ohm-cm @Temperature 400 °C | 0.000116 ohm-cm @Temperature 752 °F |
| 0.000119 ohm-cm @Temperature 500 °C | 0.000119 ohm-cm @Temperature 932 °F |
| 0.000121 ohm-cm @Temperature 600 °C | 0.000121 ohm-cm @Temperature 1110 °F |
| 0.000123 ohm-cm @Temperature 700 °C | 0.000123 ohm-cm @Temperature 1290 °F |
| 0.000125 ohm-cm @Temperature 800 °C | 0.000125 ohm-cm @Temperature 1470 °F |
| 0.000126 ohm-cm @Temperature 900 °C | 0.000126 ohm-cm @Temperature 1650 °F |
| 0.000128 ohm-cm @Temperature 1000 °C | 0.000128 ohm-cm @Temperature 1830 °F |
| 0.000129 ohm-cm @Temperature 1100 °C | 0.000129 ohm-cm @Temperature 2010 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 16.0 µm/m-°C @Temperature 20.0 - 250 °C | 8.89 µin/in-°F @Temperature 68.0 - 482 °F |
| 17.0 µm/m-°C @Temperature 20.0 - 500 °C | 9.44 µin/in-°F @Temperature 68.0 - 932 °F |
| 18.0 µm/m-°C @Temperature 20.0 - 750 °C | 10.0 µin/in-°F @Temperature 68.0 - 1380 °F |
| 19.0 µm/m-°C @Temperature 20.0 - 1000 °C | 10.6 µin/in-°F @Temperature 68.0 - 1830 °F |
Specific Heat Capacity | 0.500 J/g-°C @Temperature 200 °C | 0.120 BTU/lb-°F @Temperature 392 °F |
| 0.500 J/g-°C @Temperature 20.0 °C | 0.120 BTU/lb-°F @Temperature 68.0 °F |
| 0.500 J/g-°C @Temperature 100 °C | 0.120 BTU/lb-°F @Temperature 212 °F |
| 0.510 J/g-°C @Temperature 300 °C | 0.122 BTU/lb-°F @Temperature 572 °F |
| 0.540 J/g-°C @Temperature 400 °C | 0.129 BTU/lb-°F @Temperature 752 °F |
| 0.570 J/g-°C @Temperature 500 °C | 0.136 BTU/lb-°F @Temperature 932 °F |
| 0.600 J/g-°C @Temperature 600 °C | 0.143 BTU/lb-°F @Temperature 1110 °F |
| 0.620 J/g-°C @Temperature 700 °C | 0.148 BTU/lb-°F @Temperature 1290 °F |
| 0.640 J/g-°C @Temperature 800 °C | 0.153 BTU/lb-°F @Temperature 1470 °F |
| 0.670 J/g-°C @Temperature 900 °C | 0.160 BTU/lb-°F @Temperature 1650 °F |
| 0.700 J/g-°C @Temperature 1000 °C | 0.167 BTU/lb-°F @Temperature 1830 °F |
| 0.730 J/g-°C @Temperature 1100 °C | 0.174 BTU/lb-°F @Temperature 2010 °F |
Thermal Conductivity | 13.0 W/m-K @Temperature 20.0 °C | 90.2 BTU-in/hr-ft²-°F @Temperature 68.0 °F |
| 14.0 W/m-K @Temperature 100 °C | 97.2 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 15.0 W/m-K @Temperature 200 °C | 104 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 16.0 W/m-K @Temperature 300 °C | 111 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 18.0 W/m-K @Temperature 400 °C | 125 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 19.0 W/m-K @Temperature 500 °C | 132 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 21.0 W/m-K @Temperature 600 °C | 146 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 22.0 W/m-K @Temperature 700 °C | 153 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 24.0 W/m-K @Temperature 800 °C | 167 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 25.0 W/m-K @Temperature 900 °C | 174 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 26.0 W/m-K @Temperature 1000 °C | 180 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 28.0 W/m-K @Temperature 1100 °C | 194 BTU-in/hr-ft²-°F @Temperature 2010 °F |
Melting Point | 1390 °C | 2530 °F |
Maximum Service Temperature, Air | 1100 °C | 2010 °F |
|
Optical Properties | Metric | English | Comments |
---|
Emissivity (0-1) | 0.88 | 0.88 |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.10 % | <= 0.10 % |
Chromium, Cr | 18 - 21 % | 18 - 21 % |
Iron, Fe | >= 38.4 % | >= 38.4 % |
Manganese, Mn | <= 1.0 % | <= 1.0 % |
Nickel, Ni | 34 - 37 % | 34 - 37 % |
Silicon, Si | 1.6 - 2.5 % | 1.6 - 2.5 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.