MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Evonik Vestamid® L2123 Plasticized Nylon 12
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: Description: High-viscosity, plasticized, heat- and light-stabilized, with processing aid, increased low-temperature impact strength

Applications: Tubing and coils for air brake lines, with high cold impact strength, meets SAE J844, ISO 7628, and DIN 74323/74324

Information provided by degussa.

Evonik Industries is the successor company to Degussa.

Key Words: PA12-P, EHL,22-004
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.03 g/cc0.0372 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.60 %
@Thickness 1.00 mm,
Temperature 23.0 °C
0.60 %
@Thickness 0.0394 in,
Temperature 73.4 °F
50% R.H.; ISO 62
Linear Mold Shrinkage 0.012 cm/cm0.012 in/in127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2)
Linear Mold Shrinkage, Transverse 0.015 cm/cm0.015 in/in127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2)
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 24.0 MPa3480 psiISO 527-1/2
Elongation at Break >= 50 %>= 50 %ISO 527-1/2
Elongation at Yield 32 %32 %ISO 527-1/2
Tensile Modulus 0.370 GPa53.7 ksiISO 527-1/2
Charpy Impact Unnotched  NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 11.5 J/cm²
@Temperature 23.0 °C
54.7 ft-lb/in²
@Temperature 73.4 °F
Partial Break; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+12 ohm-cm1.00e+12 ohm-cmIEC 60093
Dielectric Constant  3.6
@Frequency 1e+6 Hz
3.6
@Frequency 1e+6 Hz
IEC 60250
 10
@Frequency 100 Hz
10
@Frequency 100 Hz
IEC 60250
Dielectric Strength 29.0 kV/mm737 kV/inK20/P50; IEC 60243-1
Dissipation Factor  0.11
@Frequency 1e+6 Hz
0.11
@Frequency 1e+6 Hz
IEC 60250
 0.20
@Frequency 100 Hz
0.20
@Frequency 100 Hz
IEC 60250
Comparative Tracking Index >= 600 V>= 600 VTest Solution A, 50 drops; IEC 60112
 600 V600 VTest Solution A, 100 drops; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 180 µm/m-°C
@Temperature 23.0 - 55.0 °C
100 µin/in-°F
@Temperature 73.4 - 131 °F
45x15x10 mm; ISO 11359
Melting Point 171 °C340 °FPeak Temperature; ISO 3146, ISO 11357
Deflection Temperature at 0.46 MPa (66 psi) 80.0 °C176 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 45.0 °C113 °FISO 75
Vicat Softening Point 120 °C248 °F50N; ISO 306
 165 °C329 °F10N; ISO 306
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
 
Descriptive Properties
ColorBlack
Electrolytic CorrosionA1 StepIEC 60426

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Evonik Vestamid® L2123 sw 9.7507 (as-conditioned) Nylon 12
Evonik Vestamid® LX9013 Plasticized Nylon 12
Evonik Vestamid® L2123 sw 9.7507 (dry properties) Nylon 12
Evonik Vestamid® L2140 sw 9.7504 (as-conditioned) Nylon 12
Evonik Vestamid® L2140 sw 9.7504 (dry properties) Nylon 12

PHULA34 / 47394

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.