MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

Carbon Printers EPU 40 Elastomeric Polyurethane
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polyurethane, TP

Material Notes: EPU 40 is a high performance polyurethane elastomer that is a good choice for applications where high elasticity and tear resistance are needed.

Information provided by Carbon®

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³liquid resin
 1.025 g/cc0.03703 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6868instant; ASTM D2240
 64
@Time 5.00 sec
64
@Time 0.00139 hour
ASTM D2240
Tensile Strength, Ultimate 7.70 MPa1120 psiDie-C Shape, 500 mm/min; ASTM D412
Tensile Stress  1.90 MPa
@Strain 50 %
276 psi
@Strain 50 %
Die-C Shape, 500 mm/min; ASTM D412
 3.00 MPa
@Strain 100 %
435 psi
@Strain 100 %
Die-C Shape, 500 mm/min; ASTM D412
 5.50 MPa
@Strain 200 %
798 psi
@Strain 200 %
Die-C Shape, 500 mm/min; ASTM D412
Elongation at Break >= 250 %>= 250 %Die-C Shape, 500 mm/min; ASTM D412
Resilience 2929[%], Bayshore Rebound; ASTM D2632
Tear Strength 23.0 kN/m131 pliDie-C (die cut); ASTM D624
Abrasion 170170[mm3], Relative Abrasion Volume Loss; ISO 4649 A
Compression Set 23 %
@Temperature 23.0 °C,
Time 259000 sec
23 %
@Temperature 73.4 °F,
Time 72.0 hour
ASTM D395-B
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 3.9
@Frequency 1e+6 Hz
3.9
@Frequency 1e+6 Hz
ASTM D150
Dissipation Factor 0.031
@Frequency 1e+6 Hz
0.031
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 8.00 °C46.4 °FDMA, tan(d); ASTM D4065

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PCARBP008 / 255840

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.