MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Special Metals INCOLOY® 25-6MO Super Austenitic Stainless Steel (UNS N08926)
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: A super-austenitic containing 6% molybedenum and offering excellent corrosion-resistance to neutral and acidic environments containing chlorides or other halides, such as what is found in air pollution control and flue gas desulfurization systems. The molybdenum and nitrogen content provide resistance to pitting and crevice corrosion, while copper enhances resistance to sulfuric acid. The alloy is especially suited for service in high-chloride environments such as brackish water, seawater, caustic chlorides and pulp mill bleach systems.

Data provided by the manufacturer, Special Metals.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.290 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 86
Tensile Strength 590 MPa
@Temperature 538 °C
Annealed before test
Tensile Strength, Ultimate 100000 psiAnnealed
Tensile Strength, Yield 48000 psi
@Strain 0.2 %
Annealed
 220 MPa
@Strain 0.2 %,
Temperature 538 °C
Annealed before test
Elongation at Break >= 42 %in 2 in (50 mm) or 4D; Annealed
 55 %
@Temperature 538 °C
Annealed before test
Modulus of Elasticity 188 GPafor Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ]
Poissons Ratio 0.33
Shear Modulus 77.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000800 ohm-cm
Magnetic Permeability 1.005at 200 Oersted (15.9 kA/m)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 15.18 µm/m-°C
@Temperature 25.0 - 100 °C
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ]
 16.03 µm/m-°C
@Temperature 25.0 - 300 °C
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ]
 16.56 µm/m-°C
@Temperature 25.0 - 500 °C
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ]
 17.18 µm/m-°C
@Temperature 25.0 - 700 °C
Mean for Hot Rolled and Annealed Plate [2100°F (1149°C)/1h/WQ]
Specific Heat Capacity 0.500 J/g-°C
Thermal Conductivity 11.5 W/m-K
Melting Point 1320 - 1400 °C
Solidus 1320 °C
Liquidus 1400 °C
Maximum Service Temperature, Air 1000 °Ftypical use
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.20 %
Chromium, Cr 19 - 21 %
Copper, Cu 0.50 - 1.5 %
Iron, Fe 47.3 %As remainder
Manganese, Mn <= 2.0 %
Molybdenum, Mo 6.0 - 7.0 %
Nickel, Ni 24 - 26 %
Nitrogen, N 0.15 - 0.25 %
Phosphorus, P <= 0.030 %
Silicon, Si <= 0.50 %
Sulfur, S <= 0.010 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Industeel URANUS® B26 6 Mo High Performance Super-Austenitic Stainless Steel with PREN = 43
Carlson 926 Mo Austenitic Stainless Steel
Special Metals INCOLOY® 25-6HN Super-Austenitic Stainless Steel
ATI Allegheny Ludlum Stainless Steel AL-6XN® Alloy (UNS N08367), 40% Cold Work
Haynes 625 alloy, cold rolled and 1050°C mill-annealed sheet

NINCO00 / 17433

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.