MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Eneos 3400B TPE
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Characteristics:
  • Original crystalline pseudo-crosslinkage structure
  • Excellent rubber elasticity (compression set) equivalent to that of crosslinked rubbers
  • Uniform closed cell and high expansion ratio obtained as TPO foams
  • Crosslinking agent free , clean elastomer
Typical Applications:
  • Packing, Seals, etc.

ENEOS has acquired the elastomer product lines from JSR Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.880 g/cc0.880 g/ccISO 1183
Melt Flow  3.0 g/10 min
@Load 5.00 kg,
Temperature 230 °C
3.0 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ISO 1133
 14 g/10 min
@Load 9.99 kg,
Temperature 230 °C
14 g/10 min
@Load 22.0 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 33
@Time 15.0 sec
33
@Time 0.00417 hour
ISO 868
Tensile Strength 4.50 MPa653 psiJIS K6251
Elongation at Break >= 1000 %>= 1000 %JIS K6251
100% Modulus 0.700 MPa102 psiISO 37
Tear Strength 22.0 kN/m126 pliISO 34 B (a)
Compression Set 41 %
@Temperature 70.0 °C,
Time 79200 sec
41 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
Shrinkage 0.60 %0.60 %JSR Method
 
Optical PropertiesMetricEnglishComments
Gloss 17 %17 %ISO 2813

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PJSRC8134 / 295450

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.