MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LyondellBasell Hifax TRC 277P G14008 Polypropylene, Talc Filled copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: Hifax polypropylene resins based on the Catalloy process are used in applications such as building and construction (e.g., single-ply roofing), industrial applications (e.g., wire and cable), and automotive industries. Hifax priovides good processability, excellent impact resistance, a broad range of stiffness from very soft to rigid products, high temperature resistance and low linear coefficient of thermal expansion.

Hifax TRC 277P G14008 is a 16% talc filled PP copolymer, with good impact/stiffness balance, good UV resistance and low CLTE (Coefficient of Linear Thermal Expansion). Product is available as a customized color matched, pellet form. Its formula is improved to offer better aspect especially on tiger stripes. This grade is delivered in G14008 color version. Applications: Exterior Automotive Applications.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.01 g/cc0.0365 lb/in³ISO 1183-1A
Melt Flow 21 g/10 min
@Load 2.16 kg,
Temperature 230 °C
21 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 21.0 MPa3050 psiISO 527-1,-2
Flexural Modulus 1.80 GPa261 ksitech. A; ISO 178/A1
Izod Impact, Notched (ISO)  4.00 kJ/m²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1A
 35.0 kJ/m²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 52.0 °C126 °FB50; ISO 306
 
Descriptive Properties
Processing MethodInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEQT7352 / 218989

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.