MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

A. Schulman DuraGrip™ DGR 6030 NC/BK Thermoplastic Elastomer (TPE)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Olefinic Elastomer (TPO)

Material Notes: DuraGrip® DGR 6030 NC/BK are designed to be general purpose Thermoplastic Elastomers (TPE) that are easy to use in injection molding and extrusion processes. DGR 6030 NC/BK have an excellent soft touch feel, will bond to olefinics, and are available in FDA compliant formulations. DuraGrip® is not hygroscopic and under normal conditions does not require drying.

Information provided by Advanced Polymer Alloys

Former product line of Advanced Polymer Alloys (APA), acquired by A. Schulman in 2014.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.990 g/cc0.990 g/ccASTM D471; ISO 2781
Viscosity 129000 cP
@Shear Rate 300 1/s,
Temperature 190 °C
129000 cP
@Shear Rate 300 1/s,
Temperature 374 °F
ASTM D3835
Linear Mold Shrinkage  0.022 cm/cm
@Thickness 3.17 mm
0.022 in/in
@Thickness 0.125 in
 0.028 cm/cm
@Thickness 1.59 mm
0.028 in/in
@Thickness 0.0625 in
Linear Mold Shrinkage, Transverse  0.013 cm/cm
@Thickness 1.59 mm
0.013 in/in
@Thickness 0.0625 in
 0.016 cm/cm
@Thickness 3.17 mm
0.016 in/in
@Thickness 0.125 in
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 3333Time of 5 seconds; ASTM D2240; ISO 48
Tensile Strength, Ultimate 3.9841 MPa577.85 psiAfter 7 days at 100°C; ASTM D412 ISO 37
 4.2468 MPa615.95 psiAfter 7 days at 70°C; ASTM D412 ISO 37
 4.38 MPa635 psiASTM D412; ISO 37
Elongation at Break 485 %485 %After 7 days at 100°C; ASTM D412 ISO 37
 500 %500 %ASTM D412; ISO 37
 515 %515 %After 7 days at 70°C; ASTM D412 ISO 37
Modulus of Elasticity 0.000986 GPa0.143 ksiAfter 7 days at 70°C; ASTM D412 ISO 37
 0.00103 GPa0.150 ksiAfter 7 days at 100°C; ASTM D412 ISO 37
100% Modulus 1.05 MPa
@Strain 100 %
153 psi
@Strain 100 %
ASTM D412; ISO 37
Graves Tear Strength 14.2 kN/m
@Temperature 23.9 °C
81.0 pli
@Temperature 75.0 °F
Die C; ASTM D624
Taber Abrasion, mg/1000 Cycles 140140Cs-17 Wheel, 1000 g Load; ASTM D3389
Compression Set  33 %
@Temperature 70.0 °C
33 %
@Temperature 158 °F
22 hrs.; ASTM D395; ISO 815
 53 %
@Temperature 100 °C
53 %
@Temperature 212 °F
22 hrs.; ASTM D395; ISO 815
 10 %
@Temperature 24.0 °C,
Time 79200 sec
10 %
@Temperature 75.2 °F,
Time 22.0 hour
ASTM D395; ISO 815
Tensile Set 5.0 %5.0 %100% Tension; ASTM D412
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -67.2 °C-89.0 °FASTM D746; ISO 812
 
Processing PropertiesMetricEnglishComments
Processing Temperature 204 °C400 °F
Rear Barrel Temperature 188 - 199 °C370 - 390 °F
Middle Barrel Temperature 199 - 210 °C390 - 410 °F
Front Barrel Temperature 216 - 227 °C420 - 440 °F
Nozzle Temperature 204 - 221 °C400 - 430 °F
Melt Temperature 199 - 221 °C390 - 430 °F
Mold Temperature 43.3 - 54.4 °C110 - 130 °F
Injection Pressure 1.03 - 3.45 MPa150 - 500 psi
Cycle Time - Injection 0.50 - 2.0 sec0.50 - 2.0 secboost
Screw Speed 25 - 100 rpm25 - 100 rpm
Cure Time 0.167 - 0.333 min0.00278 - 0.00556 hourCooling Time
 
Descriptive Properties
Fluid Resistance - Volume Change, % (ASTM D471)22After 7 Days in ASTM Ref. Fuel No. B at 75°F (24°C)
 6After 7 Days in ASTM Oil No.1 at 212°F (100°C)
 70After 7 Days in IRM 903 Oil No.3 at 212°F (100°C)
 -9After 7 Days in Water at 212°F (100°C)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman DuraGrip™ DGR 6040 NC/BK Thermoplastic Elastomer (TPE)
Overview of materials for Thermoplastic Olefinic Elastomer (TPO)
Teknor Apex Sarlink® 3135 Thermoplastic Elastomer
A. Schulman DuraGrip™ DGR 6080 NC/BK Thermoplastic Elastomer (TPE)
A. Schulman DuraGrip™ DGR 6050 NC/BK Thermoplastic Elastomer (TPE)

PAPA031 / 24098

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.