MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV X5745B Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 5700B Series are highly engineered extrusion-grade thermoplastic vulcanizates with outstanding UV stability designed for demanding automotive interior and exterior sealing applications, including glass run channels, waistbelts, weather strips, seals and other profiles. This product is a medium hardness, low density, high performance grade with low fogging and excellent color retention and elastic properties.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Additive: UV Stabilizer

Features: Chemical Resistant; Medium Hardness; Low Density; UV Resistant

Uses: Automotive Applications; Automotive Exterior Parts; Rubber Replacement

RoHS Compliance: RoHS Compliant

Automotive Specifications: DAIMLER DBL 5562.30 Color: Black; VAG VW501 23 Color: Black

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ISO 1183
Viscosity 280 cP
@Shear Rate 206 1/s,
Temperature 200 °C
280 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  44
@Time 5.00 sec
44
@Time 0.00139 hour
Extruded; ISO 868
 46
@Time 5.00 sec
46
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength at Break 3.00 MPa435 psiFlow; ISO 37
 4.30 MPa624 psiAcross Flow; ISO 37
 4.00 MPa
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
580 psi
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air at 168 hr; ISO 188
 4.39 MPa
@Treatment Temp. 150 °C,
Time 605000 sec
636 psi
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air at 168 hr; ISO 188
Tensile Stress at Strain  1.20 MPa
@Strain 100 %
174 psi
@Strain 100 %
Across Flow; ISO 37
 2.10 MPa
@Strain 100 %
305 psi
@Strain 100 %
Flow; ISO 37
 1.20 MPa
@Strain 100 %,
Treatment Temp. 135 °C
174 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
 1.21 MPa
@Strain 100 %,
Treatment Temp. 150 °C
176 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
Elongation at Break 230 %230 %Flow; ISO 37
 540 %540 %Across Flow; ISO 37
 605 %
@Treatment Temp. 150 °C,
Time 605000 sec
605 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air at 168 hr; ISO 188
 616 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
616 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air at 168 hr; ISO 188
Tear Strength 17.0 kN/m97.0 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  13 %
@Temperature 22.8 °C,
Time 79200 sec
13 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 26 %
@Temperature 70.0 °C,
Time 79200 sec
26 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 42 %
@Temperature 125 °C,
Time 252000 sec
42 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
E-Polymers EFLEX® V2045 SEBS/TPV
Chengdu Polyster 4502 High Performance Grade TPV
Barlog Plastics KEBAFLEX E 50.1 TPE-V, Shore A50
Barlog Plastics KEBAFLEX E 45.1 TPE-V, Shore A45
Barlog Plastics KEBAFLEX E 40.1 TPE-V, Shore A40

PTEKNQ1210 / 237701

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.