MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Park Aerospace Nelcote® E-763 Epoxy Prepreg, 7781 E-Glass Reinforced
Categories: Polymer; Thermoset; Epoxy

Material Notes: Nelcote® E-763 is a modified epoxy system with a nominal 250°F cure temperature. E-763 provides a transparent resin surface on the finished part which gives finished part surfaces a cosmetic attractive finish.

Key Features and Benefits:

  • Good low pressure consolidation
  • Excellent handling characteristics and out-time
  • Clear surface finish for excellent cosmetic appearance on finished parts
  • 250°F cure epoxy system

Applications/Qualifications:

  • Industrial Applications
  • Recreational Applications

Information provided by Park Electrochemical Corp.

Key Words: EP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatiles <= 1.5 %
@Temperature 135 °C
<= 1.5 %
@Temperature 275 °F
8 min
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 427 MPa
@Temperature 23.9 °C
62000 psi
@Temperature 75.0 °F
0° Direction, Dry; Oven Cure 250°F, 90 min; ASTM D638
Tensile Modulus 25.5 GPa
@Temperature 23.9 °C
3700 ksi
@Temperature 75.0 °F
0° Direction, Dry; Oven Cure 250°F, 90 min; ASTM D3039
Flexural Strength  593 MPa
@Temperature 71.1 °C
86000 psi
@Temperature 160 °F
Dry; Oven Cure 250°F, 90 min; ASTM D790
 662 MPa
@Temperature 23.9 °C
96000 psi
@Temperature 75.0 °F
Dry; Oven Cure 250°F, 90 min; ASTM D790
Flexural Modulus  23.4 GPa
@Temperature 23.9 °C
3400 ksi
@Temperature 75.0 °F
Dry; Oven Cure 250°F, 90 min; ASTM D790
 23.4 GPa
@Temperature 71.1 °C
3400 ksi
@Temperature 160 °F
Dry; Oven Cure 250°F, 90 min; ASTM D790
Compressive Strength  414 MPa
@Temperature 71.1 °C
60000 psi
@Temperature 160 °F
Dry; Oven Cure 250°F, 90 min; ASTM D695
 517 MPa
@Temperature 23.9 °C
75000 psi
@Temperature 75.0 °F
Dry; Oven Cure 250°F, 90 min; ASTM D695
Compressive Modulus  23.4 GPa
@Temperature 71.1 °C
3400 ksi
@Temperature 160 °F
Dry; Oven Cure 250°F, 90 min; ASTM D695
 25.5 GPa
@Temperature 23.9 °C
3700 ksi
@Temperature 75.0 °F
Dry; Oven Cure 250°F, 90 min; ASTM D695
Shear Strength  50.3 MPa
@Temperature 71.1 °C
7300 psi
@Temperature 160 °F
Short-Beam, Dry; Oven Cure 250°F, 90 min; ASTM D2344
 62.7 MPa
@Temperature 23.9 °C
9100 psi
@Temperature 75.0 °F
Short-Beam, Dry; Oven Cure 250°F, 90 min; ASTM D2344
 
Processing PropertiesMetricEnglishComments
Gel Time 2.00 - 6.00 min2.00 - 6.00 min
Shelf Life 6.00 Month
@Temperature -17.8 °C
6.00 Month
@Temperature 0.000 °F
 
Descriptive Properties
Prepreg Resin Content (%)36-44
Resin Flow (%)7-21275°F, 15psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Park Aerospace Nelcote® E-746 Epoxy Prepreg, 7781 E-Glass Reinforced

PPARK027 / 89299

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.