MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Evonik VESTAMID® LX9043 NC Nylon 12
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: VESTAMID® LX9043 NC is a semi-crystalline, low-viscosity molding compound based on PA12, from which various hollow articles can be produced by rotational molding. The polyamide 12 molding compound is especially suitable for industrial and technical applications with requirements for the manufacture of plastic products of different sizes. The semi-crystalline molding compound absorbs only small amounts of water. Components made from it therefore exhibit excellent dimensional stability under varying ambient humidity. VESTAMID® LX9043 NC is supplied as cylindrical granules, ready for processing, in moisture-proof bags. In the undamaged original packaging, the product has a shelf life of at least 2 years if stored in dry rooms at temperatures not exceeding 30°C. Pigmentation may affect values. Preliminary data sheet.
Dry properties listed below
Industrial Sector: Industry and Engineering
Delivery form: Pellets, Granules
Optics: Laser transparent, Opaque
Resistance to: Heat (thermal stability)
Electrical: Insulating
Additives: Release agent, Unfilled
Applications: General purpose
Processing: Thermoforming, Rotational molding
Special Characteristics: Halogen-free, Phosphorus-free, Semi-crystalline, Low viscosity
Color: Natural color
Additives: Release agent
Delivery form: Cylindrical pellets

Information provided by Evonik.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.01 g/cc0.0365 lb/in³ISO 1183
Water Absorption 1.50 %1.50 %Sim to ISO 62
Viscosity 449 cP
@Frequency 100 Hz,
Temperature 220 °C
449 cP
@Frequency 100 Hz,
Temperature 428 °F
Melt
Linear Mold Shrinkage, Flow 0.00900 cm/cm0.00900 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0120 cm/cm0.0120 in/inISO 294-4, 2577
Melt Flow 63.0 g/10 min
@Load 5.00 kg,
Temperature 230 °C
63.0 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 70.070.0ASTM D2240
Tensile Strength at Break 62.0 MPa8990 psiISO 527
Tensile Stress 31.0 MPa
@Strain 50.0 %
4500 psi
@Strain 50.0 %
ISO 527
Tensile Strength, Yield 39.0 MPa5660 psiISO 527
Elongation at Break >= 50.0 %>= 50.0 %Nominal; ISO 527
 62.0 %62.0 %ISO 527
Elongation at Yield 13.0 %13.0 %ISO 527
Tensile Modulus 1.11 GPa161 ksiISO 527
Flexural Strength 34.0 MPa4930 psiat conv. Deflection; ISO 178
 46.0 MPa6670 psiISO 178
Flexural Modulus 1.01 GPa146 ksiISO 178
Flexural Strain at Break 8.00 %8.00 %at flexural strength; ISO 178
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
Type of failure: C; ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
Type of failure: C; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 178 °C352 °FISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 96.0 °C205 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 46.0 °C115 °FISO 75-1/-2
Vicat Softening Point  133 °C
@Load 5.10 kg
271 °F
@Load 11.2 lb
50 K/h; ISO 306
 174 °C
@Load 1.02 kg
345 °F
@Load 2.25 lb
50 K/h; ISO 306
Glass Transition Temp, Tg 40.0 °C104 °FISO 11357-1/-2
 
Processing PropertiesMetricEnglishComments
Feed Temperature 40.0 - 60.0 °C104 - 140 °F
Melt Temperature 210 - 220 °C410 - 428 °F
 220 °C428 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
 80.0 °C176 °F
Drying Temperature 70.0 - 80.0 °C158 - 176 °Fpre-drying
Dry Time 5.00 - 12.0 hour5.00 - 12.0 hourpre-drying
Moisture Content 0.0700 %0.0700 %ISO 15512
 <= 0.100 %<= 0.100 %processing humidity
Back Pressure 5.00 - 10.0 MPa725 - 1450 psi
 
Descriptive Properties
ColorNatural Color
Flexural stress at breakNMPa, ISO 178

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEVONIK7928 / 325060

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.