MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Ensinger ENSIFIDE® PPS (Polyphenylene Sulfide) - Extruded Products  (discontinued **)
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes: ENSIFIDE is a high performance thermoplastic that combines good mechanical properties with excellent thermal and chemical resistance properties. There is no known solvent that dissolves ENSIFIDE at temperatures below 392°F. Its low ionic impurities make it an excellent choice for applications where low outgassing and high purity are a concern.

Uses: ENSIFIDE's excellent thermal and chemical resistance along with its low ionic impurities make it an excellent choice for applications requiring low outgassing and high purity. ENSIFIDE is typically used in the automotive, electrical/electronic, industrial, mechanical, appliance and semiconductor industries.

Ensifide grades have been replaced by Tecatron. Information Provided by Ensinger Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.0488 lb/in³ASTM D792
Water Absorption 0.020 %at 24 hours; ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 104ASTM D785
Tensile Strength, Yield 8700 psiASTM D638
Elongation at Break 4.0 %ASTM D638
Tensile Modulus 480000 psiASTM D638
Flexural Strength 17400 psiASTM D790
Flexural Modulus 435000 psiASTM D790
Izod Impact, Notched 0.500 ft-lb/inASTM D256
Coefficient of Friction, Dynamic 0.2440 psi, 50 fpm; ASTM D3702
K (wear) Factor 540 x 10-10 in³-min/ft-lb-hr40 psi, 50 fpm; ASTM D3702
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmASTM D257
Dielectric Constant 3.0
@Frequency 60 Hz
ASTM D150
Dissipation Factor 0.00010
@Frequency 60 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 40.0 µin/in-°F
@Temperature 20.0 °C
ASTM D696
Thermal Conductivity 2.08 BTU-in/hr-ft²-°FASTM C177
Melting Point 540 °FASTM D2133
Maximum Service Temperature, Air 338 °FLong Term
Deflection Temperature at 0.46 MPa (66 psi) 400 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 220 °FASTM D648
Flammability, UL94 V-0

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ensinger Tecatron® XP-79 Compression Molded PPS Compound, 70% PTFE Filled Seal Material
Ensinger Tecatron® XP-83 Compression Molded PPS Compound, Filled with 10% PTFE, 10% Graphite and 15% Carbon Fiber
Ensinger TECATRON™ PPS Polyphenylene sulfide (PPS)
Albis Plastics Tedur® L V 9900-1 PPS, Unreinforced
Mitsubishi Chemical Advanced Materials Techtron™ 1000 PPS Extruded Polyphenylene Sulfide

PENS00 / 35971

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.