MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
GEHR Plastics PSU Polysulfone
Categories: Polymer; Thermoplastic; Polysulfone (PSU)

Material Notes: Polysulfone shows great thermal stability. It possesses a high mechanical strength, very good dielectric properties and hydrolysis resistance and a high radiation resistance. PSU has a low notch impact strength.

Properties:

  • high impact strength
  • high strength and rigidity
  • very good dimensional stability
  • high chemical stability
  • high resistance to all kinds of radiation
  • self-extinguishing
  • repeated sterilization
  • not weather resistant
Applications include parts for microwave ovens, blow dryers, parts for humidifiers, food industry, pump wheels, insulators, and medical industry.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.24 g/ccISO 1183
Moisture Absorption at Equilibrium 0.30 %ISO 62
Water Absorption at Saturation 0.80 %ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 84ISO 868
Ball Indentation Hardness 167 MPaISO 2039
Tensile Strength, Yield 89.0 MPaISO 527
Elongation at Break >= 10 %ISO 527
Elongation at Yield 5.0 %ISO 527
Modulus of Elasticity 2.68 GPaISO 527
Charpy Impact Unnotched 170 kJ/m²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 3.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+13 ohmIEC 60093
Dielectric Constant 3.1
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 42.0 kV/mmIEC 60243-1
Dielectric Loss Index 0.0055
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 125 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 55.0 µm/m-°CISO 11359
Thermal Conductivity 0.250 W/m-K
@Temperature 20.0 °C
ISO 22007-4
Melting Point 188 °CDIN EN ISO 3146
Maximum Service Temperature, Air 160 °CUL 746B
Deflection Temperature at 0.46 MPa (66 psi) 181 °CISO 75
Deflection Temperature at 1.8 MPa (264 psi) 169 °CISO 75
Minimum Service Temperature, Air -100 °CUL 746B
Glass Transition Temp, Tg 188 °CDIN EN ISO 3146
Flammability, UL94 V-0test results without UL registration; UL 94
Oxygen Index 32 %ASTM D2863
 
Compliance PropertiesOriginal ValueComments
FDA YesPhysiological indifference
 
Descriptive Properties
Acid Resistanceyes
Aromatic Resistanceyes
Bondabilityyes
CKW Resistancelimited
Colornatural
Hydrocarbonate Resistanceyes
Hydroxide Resistanceyes
Ketone Resistanceyes
Physiological indifferenceyes, EEC
Resistance Against Hot Wateryes
UV Stabilizationno

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polysulfone (PSU)
Overview of materials for Polyethersulfone (PES)
BASF Ultrason® E 1010 PES
Overview of materials for Polycarbonate, Molded
Afton Plastics 450G PEEK Polyetheretherketone

PGEHR032 / 79869

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.