MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Braskem Pluris 9300 LLDPE Blown Film Extrusion Polyethylene Quatropolymer  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade

Material Notes: Pluris 9300 is a Quatropolymer produced with Spherilene technology and is a LLDPE with unique properties, such as high stiffness associated with toughness. It is easier to process than conventional LLDPE with the same melt index and shows very good bubble stability. Films obtained with this product have very low gel values. It contains processing aid, antioxidant, and antiblock additives. Its applications include: heavy-duty bags, liners, LDPE and HDPE blends, and packages for general use.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.919 g/cc0.0332 lb/in³ASTM-1505
Melt Flow 0.55 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.55 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM-D1238
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 890 %890 %ASTM-D882
Film Elongation at Break, TD 1110 %1110 %ASTM-D882
Elmendorf Tear Strength MD 230 g230 gASTM-D1922
Elmendorf Tear Strength TD 550 g550 gASTM-D1922
Elmendorf Tear Strength, MD 6.05 g/micron154 g/milASTM-D1922
Elmendorf Tear Strength, TD 14.47 g/micron367.5 g/milASTM-D1922
Dart Drop 3.95 g/micron100 g/milASTM-D1709
Dart Drop Test 150 g0.331 lbASTM-D1709
Film Tensile Strength at Break, MD 50.0 MPa7250 psiASTM-D882
Film Tensile Strength at Break, TD 40.0 MPa5800 psiASTM-D882
1% Secant Modulus, MD 270 MPa39200 psiASTM-D882
1% Secant Modulus, TD 310 MPa45000 psiASTM-D882
 
Optical PropertiesMetricEnglishComments
Haze 18 %18 %ASTM-D1003
Gloss 71 %71 %Angle 60°; ASTM-D2457

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem LL4405S Blown Film Extrusion Linear Low Density Polyethylene
Braskem LL318 LLDPE Linear Low Density Extrusion Polyethylene
Braskem LL 218 LLDPE Cast Film Extrusion Polyethylene
Braskem LL 118 LLDPE Blown Film Extrusion Polyethylene
Braskem HE150 HDPE Monofilament Polyethylene Copolymer

PBRAS857 / 106703

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.