MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Röchling SUSTAPEEK® CF 30 PEEK, 30% Carbon Filled
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Carbon Fiber Filled

Material Notes:
  • Low coefficient of thermal expansion
  • Very high rigidity and stiffness
  • Good dimensional stability
Product applications:
  • Electrical industry
  • Military technology
  • Precision mechanics

Information provided by Röchling.

Vendors: Ensinger TECAPEEK™ shapes are manufactured exclusively with Victrex™ PEEK polymer. The Ensinger process and Victrex resins ensure reliability, consistency, dimensional stability, and high temperature mechanical performance.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.41 g/ccASTM D792
Water Absorption 0.060 %
@Time 86400 sec
ASTM D570
Water Absorption at Saturation 0.30 %ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 102ASTM D785
Hardness, Rockwell R 124ASTM D785
Hardness, Shore D 93ASTM D2240
Tensile Strength, Yield 20000 psiASTM D638
Elongation at Break 5.0 %ASTM D638
Tensile Modulus 1.00e+6 psiASTM D638
Flexural Strength 25000 psiASTM D790
Flexural Modulus 1.30e+6 psiASTM D790
Compressive Strength 29000 psiASTM D695
Izod Impact, Notched 1.00 ft-lb/inASTM D256
Coefficient of Friction, Dynamic 0.20
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square <= 1e+05ASTM D257
Dielectric Constant 3.3
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 32.0 kV/mmASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.0 µin/in-°FASTM D696
Thermal Conductivity 6.30 BTU-in/hr-ft²-°F
Melting Point 645 °FASTM D789
Maximum Service Temperature, Air 480 °F
Deflection Temperature at 1.8 MPa (264 psi) 520 °FASTM D648
Flammability, UL94 V-0
@Thickness 3.17 mm
 
Compliance PropertiesOriginal ValueComments
FDA No
NSF No
USDA No

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
RTP Company RTP 2287 HF Polyetheretherketone (PEEK), Carbon Fiber - High Flow
RTP Company RTP 2281 HF Polyetheretherketone (PEEK), Carbon Fiber - High Flow
VICTREX™ PEEK 450CA30 30% Carbon Fiber Reinforced
RTP Company RTP 2299 X 123311 A Polyetheretherketone (PEEK) Carbon Nanotube - ESD Protection
Techmer ES HiFill® PEEK CF40 HF 40% Carbon Filled

PROCH9055 / 232758

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.