MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

SACO AEI THERMODAN® HF 0103-212 BK Black Non-halogen flame retardant compound
Categories: Polymer; Thermoplastic; Polyethylene (PE)

Material Notes: SACO AEI Polymers THERMODAN® HF 0103-212 BK is a black, non-halogen thermoplastic wire and cable compound. It is designed for use in a wide variety of jacketing applications. This compound has superior fire performance; including slow flame propagation, self-extinguishing characteristics, and low smoke production. It is suitable for use as a jacket compound for cables recognized under UL 1277 tray cables and can pass flame retardant requirements set forth under UL 1685, IEEE 1202 and FT-4. THERMODAN® HF 0103-212 BK is recognized under UL 2885 as being halogen free. It is UV resistant and RoHS compliant.

Information provided by SACO AEI Polymers, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.51 g/cc1.51 g/ccASTM D792
Melt Flow 4.0 g/10 min
@Load 21.6 kg,
Temperature 190 °C
4.0 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ASTM D1238
Storage Temperature -15.3 - -2.94 °C4.44 - 26.7 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 95
@Time 1.00 sec
95
@Time 0.000278 hour
ASTM D2240
Hardness, Shore D 55
@Time 1.00 sec
55
@Time 0.000278 hour
ASTM D2240
Tensile Strength at Break 12.4 MPa1800 psiASTM D638
 13.0 MPa
@Time 2.59e+6 sec
1890 psi
@Time 720 hour
Weather-o-meter; ASTM D638
 8.69 MPa
@Treatment Temp. 100 °C,
Time 346000 sec
1260 psi
@Treatment Temp. 212 °F,
Time 96.0 hour
Oil; ASTM D638
 16.1 MPa
@Treatment Temp. 121 °C,
Time 605000 sec
2340 psi
@Treatment Temp. 250 °F,
Time 168 hour
after thermal ageing; ASTM D638
Elongation at Break 195 %195 %ASTM D638
 166 %
@Time 2.59e+6 sec
166 %
@Time 720 hour
Weather-o-meter; ASTM D638
 137 %
@Treatment Temp. 121 °C,
Time 605000 sec
137 %
@Treatment Temp. 250 °F,
Time 168 hour
after thermal ageing; ASTM D638
 185 %
@Treatment Temp. 100 °C,
Time 346000 sec
185 %
@Treatment Temp. 212 °F,
Time 96.0 hour
Oil; ASTM D638
Flexural Modulus 0.193 GPa28.0 ksi1% secant; ASTM D790
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -19.0 °C-2.20 °FASTM D746
Oxygen Index 38 %38 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Zone 1 160 - 171 °C320 - 340 °F
Zone 2 166 - 177 °C330 - 350 °F
Zone 3 177 - 188 °C350 - 370 °F
Zone 4 177 - 188 °C350 - 370 °F
Die Temperature 188 - 199 °C370 - 390 °F
Melt Temperature 182 - 193 °C360 - 380 °F
Head Temperature 171 - 182 °C340 - 360 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSACO078 / 265508

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.