MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Lubrizol ESTANE® GP80AB Ester Based Thermoplastic Polyurethane
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Type: Estane® GP 80AB is an aromatic polyester-based thermoplastic polyurethane (TPU).

Appearance: Translucent spherical pellets

Uses: Injection molding parts

Available in Europe

Information provided by Lubrizol.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccISO 2781
Maximum Moisture Content 0.050
Melt Flow 20 - 40 g/10 min
@Load 21.6 kg,
Temperature 190 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 80ISO 868
Hardness, Shore D 30ISO 868
Tensile Strength, Ultimate 35.0 MPaISO 37
Elongation at Break 575 %ISO 37
Tensile Modulus 0.0130 GPaISO 527
50% Modulus 0.00370 GPa
@Strain 50 %
ISO 37
100% Modulus 0.00500 GPa
@Strain 100 %
ISO 37
300% Modulus 0.0130 GPa
@Strain 300 %
ISO 37
Rebound 49 %ISO 4662
Tear Strength 66.0 kN/mwith incision; ISO 34B
 95.0 kN/mwithout incision; ISO 34B
Abrasion 29mm3; ISO 4649
Compression Set 16 %
@Temperature 22.0 °C,
Time 252000 sec
ISO 815
 25 %
@Temperature 70.0 °C,
Time 86400 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 110 °CA50; ISO 306
 
Processing PropertiesOriginal ValueComments
Feed Temperature 40.0 °CInjection
Nozzle Temperature 185 - 195 °CInjection
Zone 1 180 - 190 °CInjection
Zone 2 185 - 195 °CInjection
Zone 3 190 - 200 °CInjection
Zone 4 190 - 200 °CInjection
Drying Temperature 90.0 °C
Dry Time 2.00 - 3.00 hour
Dew Point -30.0 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyester Thermoplastic Elastomer
Overview of materials for Thermoplastic Polyurethane, Elastomer, Polyester Grade
Overview of materials for Thermoplastic Olefinic Elastomer (TPO)
Overview of materials for Thermoplastic Elastomer, Melt-Processible Rubber
Seals Eastern 5353 Nitrile Rubber

PNOVEON156 / 55425

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.