MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
RTP Company EMI 2560.6 Polycarbonate/ABS Alloy (PC/ABS); Stainless Steel Fiber - Electrically Conductive - EMI/RFI/ESD Protection
Categories: Polymer; Thermoplastic; ABS Polymer; PC/ABS + Stainless Steel; Polycarbonate/ABS Alloy, Antistat/Conductive; Polycarbonate (PC)

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.22 g/ccASTM D 792
Additive Loading 6.0 %Primary Additive
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
ASTM D 955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 8400 psiASTM D 638
Elongation at Break >= 10 %ASTM D 638
Tensile Modulus 370 ksiASTM D 638
Flexural Strength 14800 psiASTM D 790
Flexural Modulus 440 ksiASTM D 790
Izod Impact, Notched 1.60 ft-lb/in
@Thickness 3.20 mm
ASTM D 256
Izod Impact, Unnotched 18.0 ft-lb/in
@Thickness 3.20 mm
ASTM D 4812
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity <= 10 ohm-cmASTM D 257
Surface Resistance <= 10000 ohmESD STM11.11
Surface Resistivity per Square <= 1e+05ASTM D 257; ESD STM11.11
Static Decay <= 0.50 secMIL-PRF-81705D, 5kV to 50 V, 12% RH; FTMS101C; 4046.1
Shielding Effectiveness 43 dB
@Thickness 2.00 mm,
Frequency 1e+9 Hz
ASTM D 4935
 43 dB
@Thickness 2.00 mm,
Frequency 1.30e+9 Hz
ASTM D 4935
 44 dB
@Thickness 2.00 mm,
Frequency 1.50e+9 Hz
ASTM D 4935
 45 dB
@Thickness 2.00 mm,
Frequency 7.00e+8 Hz
ASTM D 4935
 46 dB
@Thickness 2.00 mm,
Frequency 3.00e+8 Hz
ASTM D 4935
 46 dB
@Thickness 2.00 mm,
Frequency 5.00e+8 Hz
ASTM D 4935
 
Processing PropertiesOriginal ValueComments
Melt Temperature 470 - 525 °F
Mold Temperature 125 - 200 °F
Drying Temperature 200 °F
@Time 14400 sec
Moisture Content 0.020 %
Dew Point -20.0 °F
Injection Pressure 10000 - 15000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
RTP Company ESD 303 EM Polycarbonate (PC), Glass Fiber - ESD Protection - Static Dissipative - Easy Molding
A. Schulman SCHULAMID® 66 PTFE20 HS 20% PTFE Lubricated, Heat Stabilized Nylon 6/6
RTP Company RTP 1899 X 141360 Z Acrylic (PMMA); FDA Compliant Ingredients - Permanently Static Dissipative - ESD Protection - UV Stabilized - Transparent Grade
RTP Company ESD C 2580 FR Polycarbonate/ABS Alloy (PC/ABS), ESD Protection - Electrically Conductive - Flame Retardant
RTP Company ESD 800 HB Acetal (POM), ESD Protection - Static Dissipative

PQZRA13133 / 206028

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.