MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Norplex-Micarta SkatePlate SP530M Phenolic Paper Laminate Sheet
Categories: Polymer; Thermoset; Phenolic

Material Notes: Phenolic paper based grade for mechanical applications. Good tensile, compressive and flexural strength. This paper/phenolic composite is primarily a machining material as opposed to a punching stock. SkatePlate is designed to be used for the wear surfaces in roller skate and skateboard parks.

Information provided by Norplex-Micarta

Key Words: Paper, Phenolic, Micarta, Skate Park
Vendors: Norplex-Micarta is the leading manufacturer of high performance thermoset composite materials. We work directly with customers to manufacture the highest quality specialty sheet products, pre-pregs, rods and molded shapes, and tubes to meet demanding composite applications for our OEMs and fabricators around the world. Visit norplex-micarta.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.30 g/cc
@Thickness 12.7 mm
ASTM D792
Moisture Absorption 8.00 %
@Thickness 1.57 mm
ASTM D570 Condition D1-24/23
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 115
@Thickness 6.35 mm
ASTM D785
Tensile Strength 13000 psi
@Thickness 3.17 mm
CrossWise; ASTM D638 Condition A
 17000 psi
@Thickness 3.17 mm
LengthWise; ASTM D638 Condition A
Flexural Strength 22000 psi
@Thickness 1.57 mm
CrossWise; ASTM D790 Condition A
 25000 psi
@Thickness 1.57 mm
LengthWise; ASTM D790 Condition A
Compressive Strength 30300 psi
@Thickness 12.7 mm
Flatwise; ASTM D695 Condition A
 
Electrical PropertiesOriginal ValueComments
Dielectric Breakdown 3000 V
@Thickness 1.57 mm
ASTM D149 Condition D-48/50
 60000 V
@Thickness 1.57 mm
ASTM D149 Condition A
 
Thermal PropertiesOriginal ValueComments
UL RTI, Mechanical with Impact 150 °CUL Bulletin 746b
Flammability, UL94 HB
@Thickness 1.57 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Norplex-Micarta RT342 Phenolic Cotton Laminate Tube, NEMA C
Norplex-Micarta RTB320S Phenolic Linen Laminate Tube, NEMA LE
Norplex-Micarta RT130X Epoxy Fiber Glass Laminate Tube, NEMA FR-4
Norplex-Micarta RT342H Phenolic Cotton Laminate Tube, NEMA C
Norplex-Micarta RTB320H Phenolic Linen Laminate Tube, NEMA LE

PNORPM021 / 192778

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.