MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

18Cr-12Ni-Mo STAINLESS STEEL PLATES FOR REACTOR VESSELS (SUS 316-HP)
Categories: Metal; Ferrous Metal; Stainless Steel; Cast Stainless Steel; T 300 Series Stainless Steel

Material Notes:

Creep and rupture data provided by NIMS

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Rupture Strength  19.0 - 26.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
2760 - 3770 psi
@Temperature 1380 °F,
Time 100000 hour
 24.0 - 34.0 MPa
@Temperature 725 °C,
Time 3.60e+8 sec
3480 - 4930 psi
@Temperature 1340 °F,
Time 100000 hour
 34.0 - 43.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
4930 - 6240 psi
@Temperature 1290 °F,
Time 100000 hour
 46.0 - 54.0 MPa
@Temperature 675 °C,
Time 3.60e+8 sec
6670 - 7830 psi
@Temperature 1250 °F,
Time 100000 hour
 63.0 - 69.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
9140 - 10000 psi
@Temperature 1200 °F,
Time 100000 hour
 90.0 - 94.0 MPa
@Temperature 625 °C,
Time 3.60e+8 sec
13100 - 13600 psi
@Temperature 1160 °F,
Time 100000 hour
 136 - 137 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
19700 - 19900 psi
@Temperature 1110 °F,
Time 100000 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 316H Stainless Steel, Austenitic
AISI 316 Stainless Steel, Austenitic
316 Stainless Steel, annealed sheet
316 Stainless Steel, annealed plate
AK Steel 316 Austenitic Stainless steel

NIMS022 / 77539

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.