MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

EOS StainlessSteel 254 DMSL on EOS M 290; 60 µm Layer Thickness
Categories: Metal; 3D Printing/Additive Manufacturing Metal; Ferrous Metal; Stainless Steel

Material Notes: EOS StainlessSteel 254 is an austenitic stainless steel for extreme conditions. The high chromium, molybdenum and nitrogen alloying give excellent corrosion resistance in many difficult environments. The general pitting resistance equivalent PREN for 254 is 43 (PREN = %Cr + 3.3 X %Mo + 16 X %N).

Main Characteristics:

  • Excellent resistance to uniform, pitting and crevice corrosion
  • High resistance to stress corrosion cracking
  • Higher strength than conventional austenitic stainless steels
Typical Applications:
  • Chlorinated seawater handling equipment
  • Pulp and paper manufacturing devices
  • Chemical handling equipment

Information provided by EOS GmbH (Electro Optical Systems).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density >= 8.07 g/cc>= 0.292 lb/in³ISO 3369
Porosity 0.020 %0.020 %
Thickness 60.0 microns2.36 milLayer Thickness
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 730 MPa106000 psiAs manufactured vertical; ISO 6892-1
 800 MPa116000 psiAs manufactured horizontal; ISO 6892-1
 660 MPa
@Treatment Temp. 1180 °C,
Time 7200 sec
95700 psi
@Treatment Temp. 2160 °F,
Time 2.00 hour
Heat treated vertical; ISO 6892-1
 700 MPa
@Treatment Temp. 1180 °C,
Time 7200 sec
102000 psi
@Treatment Temp. 2160 °F,
Time 2.00 hour
Heat treated horizontal; ISO 6892-1
Tensile Strength, Yield 580 MPa84100 psiAs manufactured vertical; ISO 6892-1
 660 MPa95700 psiAs manufactured horizontal; ISO 6892-1
 360 MPa
@Treatment Temp. 1180 °C,
Time 7200 sec
52200 psi
@Treatment Temp. 2160 °F,
Time 2.00 hour
Heat treated horizontal; ISO 6892-1
 360 MPa
@Treatment Temp. 1180 °C,
Time 7200 sec
52200 psi
@Treatment Temp. 2160 °F,
Time 2.00 hour
Heat treated vertical; ISO 6892-1
Elongation at Break 30 %30 %As manufactured horizontal; ISO 6892-1
 36 %36 %As manufactured vertical; ISO 6892-1
 44 %
@Treatment Temp. 1180 °C,
Time 7200 sec
44 %
@Treatment Temp. 2160 °F,
Time 2.00 hour
Heat treated horizontal; ISO 6892-1
 48 %
@Treatment Temp. 1180 °C,
Time 7200 sec
48 %
@Treatment Temp. 2160 °F,
Time 2.00 hour
Heat treated vertical; ISO 6892-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.8 µm/m-°C
@Temperature 25.0 - 100 °C
8.22 µin/in-°F
@Temperature 77.0 - 212 °F
ASTM E228
 15.7 µm/m-°C
@Temperature 25.0 - 200 °C
8.72 µin/in-°F
@Temperature 77.0 - 392 °F
ASTM E228
 16.3 µm/m-°C
@Temperature 25.0 - 300 °C
9.06 µin/in-°F
@Temperature 77.0 - 572 °F
ASTM E228
 16.7 µm/m-°C
@Temperature 25.0 - 400 °C
9.28 µin/in-°F
@Temperature 77.0 - 752 °F
ASTM E228
 
Component Elements PropertiesMetricEnglishComments
Chromium, Cr 19.5 - 20.5 %19.5 - 20.5 %
Copper, Cu 0.50 - 1.0 %0.50 - 1.0 %
Molybdenum, Mo 6.0 - 7.0 %6.0 - 7.0 %
Nickel, Ni 17.5 - 18.5 %17.5 - 18.5 %
Nitrogen, N 0.18 - 0.25 %0.18 - 0.25 %
 
Descriptive Properties
Volume rate6.1 mm3/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NEOS948 / 280608

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.