MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Saint-Gobain Tygon® F-4040-A Fuel and Lubricant Tubing Formulation
Categories: Polymer; Thermoplastic

Material Notes: Description: Tygon® F-4040-A: A consistent performer lot after lot, Tygon® Fuel and Lubricant Tubing is the most requested fuel and lubricant tubing for a variety of applications -- from small engine fuel lines to coolant transfer. Specifically designed to handle most fuels and industrial lubricants, Tygon® Fuel and Lubricant Tubing resists the swelling and hardening caused by hydrocarbon-based fluids. This significantly reduces the risk of failure due to cracking and leakage. Its minimum extractability safeguards the liquid or vapor being transferred against adulteration. Extremely flexible (Shore A, 57), Tygon® Fuel and Lubricant Tubing simplifies installation, even in tight places. It is translucent yellow for positive identification and to allow easy flow monitoring. It is routinely used to handle gasoline, kerosene, heating oils, cutting compounds and glycol-based coolants.

Features and Benefits:
  • Resists embrittlement
  • Compatible with most hydrocarbons
  • Resistant to swelling
  • Highly flexible, easy to install
  • Specifically developed for fuels and lubricants
  • Ozone and UV light resistant
Typical applications include Small engine fuel lines, general automotive, recreational vehicles, lawn and garden equipment, coolant transfer, heating fuels, cutting compounds, polishing equipment, lubrication lines.
Information provided by Saint Gobain Performance Products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.26 g/cc1.26 g/ccASTM D792-91
Water Absorption 0.49 %0.49 %24 hours at 23°C; ASTM D570-95
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 575715 seconds; ASTM D2240-97
Tensile Strength, Yield 12.5 MPa1820 psiASTM D412-97
Elongation at Break 310 %310 %ASTM D412-97
100% Modulus 6.27 MPa
@Strain 100 %
910 psi
@Strain 100 %
ASTM D412-97
Tear Strength 29.3 kN/m167 pliInitial Tear Strength; ASTM D1004-93
Compression Set 65 %
@Temperature 70.0 °C
65 %
@Temperature 158 °F
Constant Deflection, for 22 hrs.; ASTM D395-89 Method B
Tensile Set 50 %50 %at 75% Elongation; ASTM D412-97
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 15.9 kV/mm403 kV/inASTM D149-93
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 73.9 °C165 °F
Brittleness Temperature -37.2 °C-35.0 °FASTM D746-95
 
Descriptive Properties
ColorTranslucent Yellow

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Saint-Gobain Tygon® Furon® 400 High-Purity PFA Tubing
Saint-Gobain Tygon® E-1000 Ultra-Soft Laboratory Tubing
Saint-Gobain Tygon® Chemfluor® Convoflex™ Spiral Designed Tubing Aids in Self-flushing and Cleaning
Saint-Gobain Tygon® A-60-N Drinking Water Tubing Formulation
Saint-Gobain Tygon® A-60-F I.B. Pressure Tubing Formulation for CIP and SIP cleaning and sterilization systems

PSTGQZ186 / 68700

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.