MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Domo TECHNYL® 2411GF6 PA66, 30% glass fiber, DRY
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Description: Polyamid 66, 30% glass fiber reinforce, for injection molding

Available in: Asia Pacific

Product Applications: TECHNYL® 2411GF6 used in all sectors of industry, offering an excellent combination between thermal stability and mechanical properties. This grade is widely used for: Automotive parts-Cooling fan, Shaft gear; Electrical & electronic parts-Plug, housing; and Sport, industrial, construction parts-Joint bushing, Disc. This product is available in natural & black color and in colors on request.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.38 g/ccISO 1183
Water Absorption 0.80 %
@Temperature 23.0 °C,
Time 86400 sec
ISO 62
Linear Mold Shrinkage, Flow 0.0050 cm/cm
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 185 MPaASTM D638
Elongation at Break 3.5 %ASTM D638
Flexural Strength 280 MPaASTM D790
Flexural Modulus 9500 MPaASTM D790
Izod Impact, Notched 115 J/mASTM D265
Charpy Impact, Notched 1.20 J/cm²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 6.00e+14 ohmIEC 60093
Dielectric Constant 3.75IEC60250
Dielectric Strength 40.0 kV/mmIEC 60243
Dissipation Factor 0.010IEC 60250
Comparative Tracking Index 500 VSolution B; IEC 60112
 600 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 25.0 µin/in-°F
@Temperature 23.0 - 85.0 °C
ISO 11359
Melting Point 262 °CISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 255 °CASTM D648
Flammability, UL94 HB
@Thickness 1.60 - 3.20 mm
ISO 1210
Oxygen Index 23 %ISO 4589
Glow Wire Ignition Temperature 650 °C
@Thickness 1.60 mm
IEC-60695-2-13
Glow Wire Flammability Index 650 °C
@Thickness 0.800 mm
IEC-60695-2-12
 
Processing PropertiesOriginal ValueComments
Feed Temperature 270 - 280 °C
Mold Temperature 70.0 - 100 °C
Drying Temperature 80.0 °C
Moisture Content <= 0.20 %
 
Descriptive Properties
Compression Zone275-285°C
Fire and smoke F index2NF F16 101, I2,F3
Mixing Zone280-290°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Domo TECHNYL® 2411GF6 PA66, 30% glass fiber, Conditioned
Envalior Durethan® ECO BKV 20 FN20 000000 Nylon 6 (PA6), 20% Glass Fiber Reinforced, Dry
Unitika BV2120G30 PA66, 30% Glass Fiber Reinforced, Flame Retardant, Dry
Domo TECHNYL® 2412GHF8 PA66, 40% glass fiber, DRY
Domo TECHNYL® eXten D247 F Nylon 66 & 610

PRHOD570 / 137801

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.