MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Syensqo (Solvay Specialty Polymers) KetaSpire® XT-920 GF30 PEEK, 30% glass fiber
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Glass Fiber Filled

Material Notes: KetaSpire® XT-920 GF30 is a 30% glass fiber reinforced, natural color grade of the industry's first true a high-temperature PEEK. Glass fiber reinforcement provides higher strength and stiffness properties than unreinforced KetaSpire® XT-920 resin, making it suitable for structural applications needing robust mechanical properties, particularly those with service temperatures approaching 300°C.

The PEEK designation is based on the 2:1 ratio of ether-to-ketone functional groups in the polymer backbone. The material provides the exceptional chemical resistance of PEEK along with a 20°C (36°F) higher glass transition temperature and a 45°C (81°F) higher melting temperature than standard PEEK. This increase in thermal performance allows engineers to achieve higher mechanical strength for components used in higher temperature and higher pressure operating environments.

Although other high-temperature polyketones exhibit thermal properties on par with KetaSpire® XT, their chemical resistance is significantly inferior to standard PEEK and KetaSpire® XT. The material's unique combination of properties makes KetaSpire® XT well-suited for applications in oil & gas, transportation, electronics, chemical processing, and other industrial uses.

Applications: Aircraft Applications; Automotive Applications; Connectors; Electrical/Electronic Applications; Housings; Industrial Applications; Oil/Gas Applications; Pump Parts; Seals

Features: Chemical Resistant; Fatigue Resistant; Flame Retardant; Good Dimensional Stability; Good Impact Resistance; High Heat Resistance; Radiotranslucent; Steam Resistant

Information provided by Solvay Specialty Polymers.

Vendors: Drake extrudes shapes and machines and injection molds parts in Torlon® PAI, PEEK, PAEK, Ryton PPS and Ultem PEI. It also machines Vespel® PI. Innovations include cryogenic CryoDyn® CT-200 shapes as a PCTFE alternative; efficient Seamless Tube® and the largest extruded rod diameters to >254mm and plate thicknesses to > 100mm. Certified to ISO 9001:2015 and AS9100D. Visit www.DrakePlastics.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.51 g/cc0.0546 lb/in³ASTM D792
Viscosity 670 cP
@Shear Rate 1000 1/s,
Temperature 420 °C
670 cP
@Shear Rate 1000 1/s,
Temperature 788 °F
Melt; ASTM D3835
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cm
@Thickness 2.00 mm
0.0030 - 0.0050 in/in
@Thickness 0.0787 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.010 - 0.012 cm/cm
@Thickness 2.00 mm
0.010 - 0.012 in/in
@Thickness 0.0787 in
ASTM D955
Melt Flow 3.5 g/10 min
@Load 2.16 kg,
Temperature 420 °C
3.5 g/10 min
@Load 4.76 lb,
Temperature 788 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 101101ASTM D785
Hardness, Shore D 87
@Time 1.00 sec
87
@Time 0.000278 hour
ASTM D2240
Tensile Strength at Break 156 MPa22600 psi5.0 mm/min; ASTM D638
 165 MPa23900 psiType 1A, 5 mm/min; ISO 527-2
Elongation at Break 3.0 %3.0 %ISO 527-2
 3.0 %3.0 %5.0 mm/min; ASTM D638
Tensile Modulus 10.4 GPa1510 ksi5.0 mm/min; ASTM D638
 10.7 GPa1550 ksiType 1A; ISO 527-2
Flexural Strength 243 MPa35200 psiASTM D790
 258 MPa37400 psiISO 178
Flexural Modulus 9.90 GPa1440 ksiASTM D790
 10.3 GPa1490 ksiISO 178
Compressive Strength 166 MPa24100 psiASTM D695
Shear Strength 91.0 MPa13200 psiASTM D732
Izod Impact, Notched 1.10 J/cm2.06 ft-lb/inASTM D256
Izod Impact, Unnotched 9.50 J/cm17.8 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 12.0 kJ/m²5.71 ft-lb/in²ISO 180
Izod Impact, Unnotched (ISO) 56.0 kJ/m²26.6 ft-lb/in²ISO 180
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant  3.33
@Frequency 1e+6 Hz
3.33
@Frequency 1e+6 Hz
ASTM D150
 3.37
@Frequency 1000 Hz
3.37
@Frequency 1000 Hz
ASTM D150
 3.38
@Frequency 60 Hz
3.38
@Frequency 60 Hz
ASTM D150
Dielectric Strength 23.0 kV/mm
@Thickness 1.60 mm
584 kV/in
@Thickness 0.0630 in
ASTM D149
Dissipation Factor  0.0010
@Frequency 1000 Hz
0.0010
@Frequency 1000 Hz
ASTM D150
 0.0010
@Frequency 60 Hz
0.0010
@Frequency 60 Hz
ASTM D150
 0.0020
@Frequency 1e+6 Hz
0.0020
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 17.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
9.44 µin/in-°F
@Temperature -58.0 - 122 °F
ASTM E831
Melting Point 385 °C725 °FPeak; ASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 332 °C630 °FAnnealed; ASTM D648
Glass Transition Temp, Tg 170 °C338 °FDSC
Flammability, UL94  V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
 V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 405 °C761 °F
Middle Barrel Temperature 405 °C761 °F
Front Barrel Temperature 410 °C770 °F
Nozzle Temperature 410 °C770 °F
Mold Temperature 205 - 230 °C401 - 446 °F
Drying Temperature 150 °C
@Time 14400 sec
302 °F
@Time 4.00 hour
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 North America
ColorBeige
FormsPellets
Injection RateFast
ProcessingInjection Molding; Machining; Profile Extrusion
RoHS ComplianceYes
Screw Compression Ratio2.5:1.0 to 3.5:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4354 / 280154

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.