MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, OSO50 Temper flat products, rod, tube, shapes
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold workability; good forgeability. Fabricated by coining, coppersmithing, drawing and upsetting, hot forging and pressing, spinning, swaging, stamping.

Applications: downspouts, gutters, roofing, gaskets, auto radiators, busbars, nails, printing rolls, rivets, and radio parts.

Test specimens: flat products - 1mm and 6mm thicknesses, rod - 25mm OD, tube - 25mm OD x 1.65mm wall thickness, and shapes - 13mm section.

Key Words: ASTM-B-152, QQ-C-576, CDA 110 ETP, C101, ISO Cu-ETP
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.89 g/cc
 7.93 g/cc
@Temperature 1083 °C
Liquid
 8.32 g/cc
@Temperature 1083 °C
Solid
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell F 40
Tensile Strength, Ultimate 220 MPa
 235 MPa
@Temperature -40.0 °C
 260 MPa
@Temperature -75.0 °C
 285 MPa
@Temperature -120 °C
 320 MPa
@Temperature 12.0 °C
 325 MPa
@Temperature -12.0 °C
 400 MPa
@Temperature -175 °C
Tensile Strength, Yield 69.0 MPa
@Strain 0.5 %
 65.0 MPa
@Strain 0.1 %,
Temperature 0.000 °C
 70.0 MPa
@Strain 0.1 %,
Temperature -50.0 °C
 75.0 MPa
@Strain 0.1 %,
Temperature -100 °C
 80.0 MPa
@Strain 0.1 %,
Temperature -150 °C
Elongation at Break 55 %In 50 mm, rod
 40 %
@Temperature -12.0 °C
 45 %
@Temperature -120 °C
 47 %
@Temperature 12.0 °C
 48 %
@Temperature -75.0 °C
 48 %
@Temperature -40.0 °C
 57 %
@Temperature -175 °C
 45 %
@Thickness 1.00 mm
in 50 mm; tube
 50 %
@Thickness 6.00 mm
in 50 mm; shapes
Reduction of Area 70 %
@Temperature -120 °C
 74 %
@Temperature -75.0 °C
 76 %
@Temperature 12.0 °C
 77 %
@Temperature -40.0 °C
 77 %
@Temperature -175 °C
 78 %
@Temperature -12.0 °C
Modulus of Elasticity 115 GPaO60 temper
Poissons Ratio 0.33
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %UNS C37700 (forging brass) = 100%
Shear Modulus 44.0 GPaO60 temper
Shear Strength 150 MPa
Coefficient of Friction, Dynamic 0.29Sliding, with cast iron, no lubrication
 0.36Sliding, with carbon steel, no lubrication
 0.53Sliding, with glass, no lubrication
Coefficient of Friction, Static 0.53With carbon steel, no lubrication
 0.68With carbon steel, no lubrication
 1.05With cast iron, no lubrication
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000170 ohm-cm101% IACS
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 205 J/g
CTE, linear 17.0 µm/m-°C
@Temperature 20.0 - 100 °C
 17.3 µm/m-°C
@Temperature 20.0 - 200 °C
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.385 J/g-°C
Thermal Conductivity 300 W/m-K
@Temperature -268.8 °C
 300 W/m-K
@Temperature 700 °C
 370 W/m-K
@Temperature 300 °C
 380 W/m-K
@Temperature 100 °C
 388 W/m-K
@Temperature 20.0 °C
 390 W/m-K
@Temperature 0.000 °C
 400 W/m-K
@Temperature -79.0 °C
 550 W/m-K
@Temperature -196 °C
 1300 W/m-K
@Temperature -253 °C
Melting Point 1065 - 1083 °C
Solidus 1065 °CEutectic
Liquidus 1083 °C
Softening Point 360 °C
Annealing Point >= 700 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 475 - 750 °C
Hot-Working Temperature 750 - 875 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu >= 99.90 %includes Ag
Oxygen, O 0.040 %
 
Descriptive Properties
ColorReddish metallic

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, OSO25 Temper flat products, tube
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, H00 Temper flat products
Cadi C11000 ETP Standard Grade Copper
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, H01 Temper flat products
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, H02 Temper flat products

MC11000b3 / 10490

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.