MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

Clariant Natural Color Bio-based 3D Printer Filament
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Renewable/Recycled Polymer

Material Notes: Clariant’s bio-based compound was developed specifically for 3D printing with customers. It has a nicer surface finish when printed compared to PLA. End use application the material is enhanced with Hostanox® P-EPQ®, and Hostavin® ARO 8 additives.Benefits: General properties:
  • High tensile strength
  • Matte finish
Optimized benefits:
  • Reduced thermo-oxidative degradation
  • Minimized undesired yellowing due to ultraviolet radiation
Applications:
  • Reduced thermo-oxidative degradation
  • Minimized undesired yellowing due to ultraviolet radiation

Information provided by Clariant.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.21 g/cc0.0798 lb/in³ISO 1183
Melt Flow  2.2 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.2 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 10.8 g/10 min
@Load 2.16 kg,
Temperature 210 °C
10.8 g/10 min
@Load 4.76 lb,
Temperature 410 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 44.0 MPa6380 psiInjection molded, 50 mm/min; ISO 527
Tensile Strength, Yield 44.0 MPa6380 psiInjection molded, 50 mm/min; ISO 527
Elongation at Break 2.0 %2.0 %Injection molded, 50 mm/min; ISO 527
Modulus of Elasticity 2.807 GPa407.1 ksiInjection molded, 1 mm/min; ISO 527
Izod Impact, Unnotched (ISO) 75.0 kJ/m²35.7 ft-lb/in²Injection molded, brittle; ISO 180
 
Thermal PropertiesMetricEnglishComments
Melting Point 144 °C291 °FDSC; ISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 54.0 °C129 °F3D printed flat; ISO 75
Glass Transition Temp, Tg 55.0 °C131 °FDSC; ISO 11357
 
Processing PropertiesMetricEnglishComments
Processing Temperature 200 - 220 °C392 - 428 °FPrint Temperature
 
Descriptive Properties
Bed Adhesiona glass, polyimide tape, polyethylenimine (PEI), carbon fiber or surface coated with a PVA glue have proven to work
Bed Temperatureideally heated up to 70°C and in an enclosed chamber
Fan Settingslow to medium
Print Speed30-70 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Clariant Polyamide 12 3D Printer Filament

PCLAR00016 / 232093

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.