MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Parson Adhesives SONLOCK™ 3515 Anaerobic Gasket Sealant
Categories: Polymer; Adhesive; Thermoset

Material Notes: SONLOK 3515 is an anaerobic gasket sealant, which develops medium strength in a short time. The compound cures in the absence of air between close fitting metal surfaces. SONLOK 3515 is a flexible gasketing sealant which will flex with minor flange movements. Provides resistance to low pressure immediately after assembly of flanges.

Applications:

  • Typically used as a form-in-place gasket for pumps, thermostats, compressors, transmission housings and axle covers.
  • Thixotropic nature reduces the migration of liquid product after application.

Information provided by Parson Adhesives, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.10 g/cc1.10 g/cc
Brookfield Viscosity 275000 - 950000 cP275000 - 950000 cPThixotropic, RVT, Spindle 7 @ 20 rpm
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 14.0 MPa2030 psiSteel, grit blasted; ISO 6922
Compressive Strength >= 5.00 MPa
@Time 86400 sec
>= 725 psi
@Time 24.0 hour
Steel Pins & Collars; ISO 10123
Shear Strength 6.00 MPa870 psiSteel, grit based; ISO 4587
 
Thermal PropertiesMetricEnglishComments
CTE, linear 80.0 µm/m-°C44.4 µin/in-°FASTM D696 K-1
Specific Heat Capacity 0.300 J/g-°C0.0717 BTU/lb-°F
Thermal Conductivity 0.100 W/m-K0.694 BTU-in/hr-ft²-°FASTM C177
Maximum Service Temperature, Air 149 °C300 °F
Minimum Service Temperature, Air -53.9 °C-65.0 °F
Flash Point >= 93.0 °C>= 199 °F
 
Processing PropertiesMetricEnglishComments
Cure Time 15.0 - 120 min0.250 - 2.00 hourHandling, Primed Surfaces
 60.0 - 120 min1.00 - 2.00 hourHandling, Unprimed Surfaces
 
Descriptive Properties
ColorPurple
CompositionDimethacrylate ester
Diameter>0.5 mmThread/Gap Filling
Initial Strength Retained (%)100Acetone for 500 hrs at 22°C
 15Gasoline for 1000 hrs at 22°C
 160Motor Oil for 500 hrs at 125°C
 165Motor Oil for 1000 hrs at 125°C
 20Gasoline for 500 hrs at 22°C
 80Water/Glycol for 500 hrs at 87°C
 80Water/Glycol for 1000 hrs at 87°C
 85Ethanol for 1000 hrs at 22°C
 90Ethanol for 500 hrs at 22°C
 95Acetone for 1000 hrs at 22°C
 95Break Fluid for 500 hrs at 22°C
 95Break Fluid for 1000 hrs at 22°C
Solvent ContentNone

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPARSN030 / 186473

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.