MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

BNZ Materials Color CA Insulating Firebrick (French Grade)
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: BNZ produces many types of Insulating Fire Brick (IFB) for use in applications from 2,000°F (1,093°C) to 3,200°F (1,760°C). Each type is formulated to meet specific thermal and physical requirements and after firing is machined to precise tolerances. Made from high purity refractory clays and other ceramic raw materials, these IFB contain a carefully graded organic filler which is burned out during manufacture to give a uniform controlled pore structure.

Information provided by BNZ Materials Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0398 lb/in³ASTM C134
 
Mechanical PropertiesMetricEnglishComments
Compressive Strength 5.40 MPa783 psiCold Crush Strength; ASTM C133
 
Thermal PropertiesMetricEnglishComments
CTE, linear 6.30 µm/m-°C
@Temperature 20.0 - 1000 °C
3.50 µin/in-°F
@Temperature 68.0 - 1830 °F
Thermal Conductivity  0.290 W/m-K
@Temperature 200 °C
2.01 BTU-in/hr-ft²-°F
@Temperature 392 °F
ASTM C182
 0.320 W/m-K
@Temperature 400 °C
2.22 BTU-in/hr-ft²-°F
@Temperature 752 °F
ASTM C182
 0.360 W/m-K
@Temperature 600 °C
2.50 BTU-in/hr-ft²-°F
@Temperature 1110 °F
ASTM C182
 0.400 W/m-K
@Temperature 800 °C
2.78 BTU-in/hr-ft²-°F
@Temperature 1470 °F
ASTM C182
 0.450 W/m-K
@Temperature 1000 °C
3.12 BTU-in/hr-ft²-°F
@Temperature 1830 °F
ASTM C182
Maximum Service Temperature, Air 1350 °C2460 °F
Shrinkage 0.50 %
@Temperature 1350 °C,
Time 43200 sec
0.50 %
@Temperature 2460 °F,
Time 12.0 hour
Permanent Linear Change; ASTM C210
 
Descriptive Properties
Composition (%)0.4CaO + MgO
 2.4Fe2O3 + TiO2
 4Na2O + K2O
 92.4Al2O3 + SiO2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CeramTec Ziralit Zirconia Toughened Alumina (ZTA), Al2O3•ZrO2
CeramTec Sikor® S Cordierite
CeramTec Rubalit® 600 Alumina, 48%
CeramTec 433 Alumina, 99.9%
BNZ Materials Color A Insulating Firebrick (French Grade)

CBNZ923 / 149163

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.