MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

SABIC LNP™ ELCRES™ CRX1414 Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP ELCRES CRX1414 is an amorphous Polycarbonate (PC) copolymer resin that offers medium flow, high ductility in combination with excellent chemical resistance. This grade is available for custom coloring and may be an excellent candidate for a wide variety of applications that need improved chemical resistance.

Features: Enhanced Low Temperature Impact,Enhanced Chemical Resistance,Colorable,High Impact Resistance

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Density 1.19 g/cc0.0430 lb/in³ISO 1183
Water Absorption 0.20 %
@Time 86400 sec
0.20 %
@Time 24.0 hour
ISO 62-1
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.0700 %0.0700 %23°C/50% RH/24 hrs; ISO 62-4
Viscosity  9.0 cP
@Load 1.20 kg,
Temperature 300 °C
9.0 cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
 9.5 cP
@Load 1.20 kg,
Temperature 300 °C
9.5 cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ASTM D1238
Linear Mold Shrinkage, Flow 0.0040 - 0.0090 cm/cm0.0040 - 0.0090 in/inSABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0090 cm/cm0.0040 - 0.0090 in/inSABIC method
Melt Flow 10 g/10 min
@Load 1.20 kg,
Temperature 300 °C
10 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 61.0 MPa8850 psi50 mm/min; ISO 527
 63.0 MPa9140 psi50 mm/min; ASTM D638
Tensile Strength, Yield 52.0 MPa7540 psi50 mm/min; ISO 527
 54.0 MPa7830 psi50 mm/min; ASTM D638
Elongation at Break >= 100 %>= 100 %50 mm/min; ASTM D638
 >= 100 %>= 100 %50 mm/min; ISO 527
Elongation at Yield 6.0 %6.0 %50 mm/min; ASTM D638
 6.0 %6.0 %50 mm/min; ISO 527
Tensile Modulus 1.90 GPa276 ksi1 mm/min; ISO 527
 2.02 GPa293 ksi50 mm/min; ASTM D638
Flexural Strength 83.0 MPa12000 psi2 mm/min; ISO 178
 90.0 MPa13100 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.062 GPa299.1 ksi2 mm/min; ISO 178
 2.17 GPa315 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 875 J645 ft-lbASTM D256
 657 J
@Temperature -70.0 °C
485 ft-lb
@Temperature -94.0 °F
ASTM D256
 727 J
@Temperature -60.0 °C
536 ft-lb
@Temperature -76.0 °F
ASTM D256
 777 J
@Temperature -30.0 °C
573 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Unnotched NBNBASTM D4812
 NB
@Temperature -70.0 °C
NB
@Temperature -94.0 °F
ASTM D4812
Izod Impact, Notched (ISO) 63.0 kJ/m²30.0 ft-lb/in²80*10*3; ISO 180/1A
 40.0 kJ/m²
@Temperature -70.0 °C
19.0 ft-lb/in²
@Temperature -94.0 °F
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NBNB80*10*3; ISO 180/1U
 NB
@Temperature -70.0 °C
NB
@Temperature -94.0 °F
80*10*3; ISO 180/1U
Charpy Impact Unnotched NBNBEdgew 80*10*3 sp=62mm; ISO 179/1eU
 NB
@Temperature -70.0 °C
NB
@Temperature -94.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 7.00 J/cm²33.3 ft-lb/in²Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 62.0 J45.7 ft-lbASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 136 °C277 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 138 °C
@Thickness 3.20 mm
280 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 123 °C253 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 125 °C
@Thickness 3.20 mm
257 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 142 °C288 °FRate B/50; ISO 306
 143 °C289 °FRate B/50; ASTM D1525
 144 °C291 °FRate B/120; ISO 306
 146 °C295 °FRate B/120; ASTM D1525
UL RTI, Electrical 80.0 °C176 °FUL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °FUL 746B
UL RTI, Mechanical without Impact 80.0 °C176 °FUL 746B
Flammability, UL94 HB
@Thickness >=0.750 mm
HB
@Thickness >=0.0295 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 290 - 340 °C554 - 644 °F
Zone 2 280 - 330 °C536 - 626 °F
Zone 3 290 - 340 °C554 - 644 °F
Melt Temperature 290 - 340 °C554 - 644 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 12.0 hour12.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 80 %40 - 80 %
Vent Depth 0.00250 - 0.00760 cm0.000984 - 0.00299 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
Instrumented Dart Impact Ductility, 23°C100 %ASTM D3763

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80585 / 288532

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.