Physical Properties | Metric | English | Comments |
---|
Viscosity | 290 cP | 290 cP |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore D | 83 @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 83 @Treatment Temp. 71.6 °F, Time 336 hour |
| 84 @Treatment Temp. 60.0 °C, Time 28800 sec | 84 @Treatment Temp. 140 °F, Time 8.00 hour |
Tensile Strength | 46.1 MPa @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 6680 psi @Treatment Temp. 71.6 °F, Time 336 hour |
| 51.0 MPa @Treatment Temp. 60.0 °C, Time 28800 sec | 7390 psi @Treatment Temp. 140 °F, Time 8.00 hour |
Elongation at Break | 2.7 % @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 2.7 % @Treatment Temp. 71.6 °F, Time 336 hour |
| 3.0 % @Treatment Temp. 60.0 °C, Time 28800 sec | 3.0 % @Treatment Temp. 140 °F, Time 8.00 hour |
Tensile Modulus | 2.80 GPa | 406 ksi |
| 2.85 GPa | 414 ksi |
Flexural Strength | 81.4 MPa @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 11800 psi @Treatment Temp. 71.6 °F, Time 336 hour |
| 88.9 MPa @Treatment Temp. 60.0 °C, Time 28800 sec | 12900 psi @Treatment Temp. 140 °F, Time 8.00 hour |
Flexural Modulus | 2.50 GPa @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 362 ksi @Treatment Temp. 71.6 °F, Time 336 hour |
| 2.70 GPa @Treatment Temp. 60.0 °C, Time 28800 sec | 391 ksi @Treatment Temp. 140 °F, Time 8.00 hour |
Compressive Yield Strength | 81.4 MPa @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 11800 psi @Treatment Temp. 71.6 °F, Time 336 hour |
| 84.8 MPa @Treatment Temp. 60.0 °C, Time 28800 sec | 12300 psi @Treatment Temp. 140 °F, Time 8.00 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Deflection Temperature at 0.46 MPa (66 psi) | 46.7 °C @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 116 °F @Treatment Temp. 71.6 °F, Time 336 hour |
| 47.8 °C @Treatment Temp. 60.0 °C, Time 28800 sec | 118 °F @Treatment Temp. 140 °F, Time 8.00 hour |
Glass Transition Temp, Tg | 58.9 °C | 138 °F |
| 48.3 °C @Treatment Temp. 60.0 °C, Time 28800 sec | 119 °F @Treatment Temp. 140 °F, Time 8.00 hour |
| 49.4 °C @Treatment Temp. 22.0 °C, Time 1.21e+6 sec | 121 °F @Treatment Temp. 71.6 °F, Time 336 hour |
|
Processing Properties | Metric | English | Comments |
---|
Pot Life | 135 - 165 min @Load 0.100 kg | 135 - 165 min @Load 0.221 lb |
Shelf Life | 24.0 Month | 24.0 Month |
| 36.0 Month | 36.0 Month |
|
Descriptive Properties |
---|
Mix ratio | 100:27.0 |
| 100:32.0 |
| 3.13:1 |
| 3.70:1 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.