MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Pressure Seal 4825 Chloroprene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 4825 is an 80 durometer white colored Neoprene elastomer, it is formulated with FDA sanctioned materials.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 4 BC 815 A14 EO14 EO34 G21; 2 BE 815 A14 EO14

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.68 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 83
 52
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 68
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 72
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 72
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 76
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 85
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 87
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 87
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 1524 psi
 1161.3 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 1298.4 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 1431.1 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1662.7 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 1700.8 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 1763.3 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 1763.3 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Elongation, Ultimate 420 %
 320.04 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 320.04 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 359.94 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 459.9 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 490.1 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 519.96 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 550.2 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
100% Modulus 675 psi
Tear Strength 309 pliDie C; Method D 624
 337 pliDie B; Method D 624
Compression Set 38.1 %
@Temperature 100 °C,
Time 79200 sec
Solid
 49.2 %
@Temperature 100 °C,
Time 252000 sec
Solid
 51.8 %
@Temperature 100 °C,
Time 79200 sec
Plied
 60.7 %
@Temperature 100 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -29.0 °F
Shrinkage 8.4 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #1
 13.6 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 19.1 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 70.3 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 79.2 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #3
 
Descriptive Properties
ColorWhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL086 / 318296

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.