MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik 12C27 Strip Steel
Categories: Metal; Ferrous Metal; Martensitic; Special-Purpose Steel; Stainless Steel

Material Notes: Sandvik 12C27 is a martensitic stainless chromium steel with an optimized analysis for high quality professional knife applications.

After heat treatment the composition of carbon and chromium gives a unique combination of properties including:

  • Very high hardness
  • Good corrosion resistance
  • Very high wear resistance
  • This grade is suitable for:

  • Hunting and fishing knives
  • Pocket knives
  • Skate blades and ice drills
  • Information provided by Sandvik

    ASTM 420; EN 1.4034, 1.4037

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Density 7.70 g/cc
     
    Mechanical PropertiesOriginal ValueComments
    Hardness, Rockwell B <= 94.3soft annealed
     91.4 - 103.4annealed
     94.3 - 106.6cold rolled
    Hardness, Rockwell C 53.6tempering temperature- 350°C
     59.8tempering temperature- 150°C
    Hardness, Vickers <= 215soft annealed
     200 - 270annealed
     215 - 315cold rolled
    Tensile Strength <= 700 MPasoft annealed
     650 - 850 MPaannealed
     700 - 1000 MPacold rolled
     
    Component Elements PropertiesOriginal ValueComments
    Carbon, C 0.60 %
    Chromium, Cr 13.5 %
    Iron, Fe 85.1 %As Balance
    Manganese, Mn 0.40 %
    Phosphorus, P <= 0.025 %
    Silicon, Si 0.40 %
    Sulfur, S <= 0.010 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Sandvik 12C27M Strip Steel
    420 Stainless Steel
    304 Stainless Steel
    304 Stainless Steel (UNS S30400); Annealed Strip
    AISI E 52100 Steel (100Cr6, SUJ2, UNS G52986)

    NSANDV276 / 19170

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.