MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Delrin Delrin® 100T BK602 POM-I
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Toughened High Viscosity Acetal Homopolymer

Information provided by DuPont; Delrin was sold by DuPont in 2023.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.37 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.013 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.015 cm/cmISO 294-4, 2577
Melt Flow 1.7 g/10 min
@Load 2.16 kg,
Temperature 190 °C
cm³/10min Volumetric; ISO 1133
 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 54.0 MPaISO 527-1/-2
Elongation at Break >= 50 %Nominal; ISO 527-1/-2
Elongation at Yield 27 %ISO 527-1/-2
Tensile Modulus 1900 MPaISO 527-1/-2
Poissons Ratio 0.41
Charpy Impact, Notched 11.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 23.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 178 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 71.0 °CISO 75-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
IEC 60695-11-10
Flame Spread 42.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 200 °COptimum, Extrusion
 195 - 205 °CRange, Extrusion
 200 - 210 °CRange, Injection
 205 °COptimum, Injection
Mold Temperature 50.0 °COptimum, Injection
 40.0 - 60.0 °CInjection
Drying Temperature 80.0 °CInjection
 80.0 °CExtrusion
Dry Time 4.00 - 8.00 hourExtrusion, Dehumidified Dryer
 4.00 - 8.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.050 %Extrusion
 <= 0.050 %Injection
Hold Pressure 60.0 - 80.0 MPaInjection
 80.0 MPaInjection
Annealing Temperature 160 °COptional; 2 mm/min; Injection
 
Descriptive Properties
AdditivesRelease agent
Annealing time (min/mm)30Optional, Injection
Drying RecommendedyesInjection
Emissions (mg/kg)<8VDA 275
FMVSS ClassBISO 3795 (FMVSS 302)
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>POM-I<ISO 11469
PolymerPOM
Processing Hold Pressure Time (s/mm)7.5Injection
Resin IdentificationPOM-IISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Delrin Delrin® 100 BK602 POM
Delrin Delrin® 150 NC010 POM
DuPont Mobility and Materials Delrin® II150E BK602 Acetal (POM)
Delrin Delrin® 500T BK602 POM-I
DuPont Mobility and Materials Delrin® 100PE BK602 POM

PDSX5092 / 197732

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.