MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Sandvik Sanicro 30 Seamless tube and pipe
Categories: Metal; Ferrous Metal; Austenitic

Material Notes: Nickel-iron-chromium alloy, Low carbon version, UNS N08800

Sandvik Sanicro 30 is a low-carbon version of the austenitic nickel-iron-chromium alloy. It is used for steam generator tubing in nuclear stations (PWR) and other heat exchangers for temperature up to about 550°C (1020 °F) where good resistance to stress corrosion cracking and intergranular corrosion is required.

Information provided by Sandvik

UNS N08800; EN 1.4558

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.00 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 150annealed
 170slightly cold-worked
Tensile Strength, Ultimate 520 - 690 MPaannealed
 570 - 700 MPaslightly cold-worked
Tensile Strength, Yield >= 205 MPa
@Strain 0.2 %
annealed
 >= 235 MPa
@Strain 1 %
annealed
 >= 335 MPa
@Strain 0.2 %
slightly cold-worked
 >= 355 MPa
@Strain 1 %
slightly cold-worked
 >= 145 MPa
@Strain 0.2 %,
Temperature 600 °C
annealed
 >= 165 MPa
@Strain 1 %,
Temperature 600 °C
annealed
 >= 190 MPa
@Strain 0.2 %,
Temperature 200 °C
annealed
 >= 215 MPa
@Strain 1 %,
Temperature 200 °C
annealed
 >= 275 MPa
@Strain 0.2 %,
Temperature 600 °C
slightly cold-worked
 >= 285 MPa
@Strain 1 %,
Temperature 600 °C
slightly cold-worked
 >= 325 MPa
@Strain 0.2 %,
Temperature 200 °C
slightly cold-worked
 >= 335 MPa
@Strain 1 %,
Temperature 200 °C
slightly cold-worked
Elongation at Break >= 30 %2"; slightly cold-worked
 >= 30 %
@Thickness 50.8 mm
annealed
Modulus of Elasticity 200 GPa
 160 GPa
@Temperature 600 °C
 175 GPa
@Temperature 400 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000118 ohm-cm
@Temperature 600 °C
 0.0000990 ohm-cm
@Temperature 20.0 °C
 0.000108 ohm-cm
@Temperature 400 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.0 µm/m-°C
@Temperature 20.0 - 100 °C
 16.0 µm/m-°C
@Temperature 20.0 - 200 °C
 16.5 µm/m-°C
@Temperature 20.0 - 500 °C
Specific Heat Capacity 0.475 J/g-°C
@Temperature 20.0 °C
 0.515 J/g-°C
@Temperature 200 °C
 0.525 J/g-°C
@Temperature 400 °C
 0.585 J/g-°C
@Temperature 600 °C
Thermal Conductivity 12.0 W/m-K
@Temperature 20.0 °C
 16.0 W/m-K
@Temperature 200 °C
 18.0 W/m-K
@Temperature 400 °C
 23.0 W/m-K
@Temperature 600 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.30 %
Carbon, C <= 0.030 %
Chromium, Cr 20 %
Cobalt, Co <= 0.10 %
Copper, Cu <= 0.10 %
Iron, Fe 45.8 %As Balance
Manganese, Mn 0.60 %
Nickel, Ni 32 %
Phosphorus, P <= 0.020 %
Silicon, Si 0.50 %
Sulfur, S <= 0.015 %
Titanium, Ti 0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1020 Steel, cold rolled
ASTM A808 HSLA Steel, Thickness 40 - 50 mm (1.5 to 2 in.)
ASTM A500 Steel, grade A, Round Structural Tubing
ASTM A424 Steel, type I, commercial quality
ASTM A182, Grade F11, Class 1

NSANDV250 / 19144

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.