MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Toyobo GLAMIDE® T-779 Nylon-6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 40% Mineral Filled

Material Notes: GLAMIDE® is very tough and exhibits high abrasion resistance. It has a high melting point and heat resistance, has well-balanced proportions of mechanical properties, performs self-distinguishing and a specific grade approved as UL94V-0 class is provided, and it exhibits excellent chemical resistance and oil resistance. Grade T-779 is a mineral-reinforced Nylon-6 with high impact resistance. It is used for plating.

37

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.43 g/cc1.43 g/ccAbsolute Drying; ASTM-D792
Filler Content 37 %37 %
Water Absorption 0.70 %0.70 %Absolute Drying; ASTM-D570
Linear Mold Shrinkage  0.0030 - 0.0050 cm/cm
@Thickness 1.00 mm
0.0030 - 0.0050 in/in
@Thickness 0.0394 in
Absolute Drying
 0.0080 - 0.013 cm/cm
@Thickness 3.00 mm
0.0080 - 0.013 in/in
@Thickness 0.118 in
Absolute Drying
Melt Flow 10 g/10 min10 g/10 min
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 120120Absolute Drying; ASTM-D785
Tensile Strength, Ultimate  25.0 MPa
@Temperature 80.0 °C
3630 psi
@Temperature 176 °F
Practical Use; ASTM-D638
 31.0 MPa
@Temperature 80.0 °C
4500 psi
@Temperature 176 °F
Absolute Drying; ASTM-D638
 35.0 MPa
@Temperature 23.0 °C
5080 psi
@Temperature 73.4 °F
Practical Use; ASTM-D638
 65.0 MPa
@Temperature 23.0 °C
9430 psi
@Temperature 73.4 °F
Absolute Drying; ASTM-D638
 75.0 MPa
@Temperature -40.0 °C
10900 psi
@Temperature -40.0 °F
Practical Use; ASTM-D638
 80.0 MPa
@Temperature -40.0 °C
11600 psi
@Temperature -40.0 °F
Absolute Drying; ASTM-D638
Elongation at Break 16 %16 %Absolute Drying; ASTM-D638
 35 %35 %Practical Use; ASTM-D638
Flexural Strength  32.0 MPa
@Temperature 80.0 °C
4640 psi
@Temperature 176 °F
Practical Use; ASTM-D790
 48.0 MPa
@Temperature 80.0 °C
6960 psi
@Temperature 176 °F
Absolute Drying; ASTM-D790
 62.0 MPa
@Temperature 23.0 °C
8990 psi
@Temperature 73.4 °F
Practical Use; ASTM-D790
 110 MPa
@Temperature 23.0 °C
16000 psi
@Temperature 73.4 °F
Absolute Drying; ASTM-D790
 132 MPa
@Temperature -40.0 °C
19100 psi
@Temperature -40.0 °F
Practical Use; ASTM-D790
 140 MPa
@Temperature -40.0 °C
20300 psi
@Temperature -40.0 °F
Absolute Drying; ASTM-D790
Flexural Modulus  0.700 GPa
@Temperature 80.0 °C
102 ksi
@Temperature 176 °F
Practical Use; ASTM-D790
 1.10 GPa
@Temperature 80.0 °C
160 ksi
@Temperature 176 °F
Absolute Drying; ASTM-D790
 1.50 GPa
@Temperature 23.0 °C
218 ksi
@Temperature 73.4 °F
Practical Use; ASTM-D790
 4.00 GPa
@Temperature 23.0 °C
580 ksi
@Temperature 73.4 °F
Absolute Drying; ASTM-D790
 5.10 GPa
@Temperature -40.0 °C
740 ksi
@Temperature -40.0 °F
Practical Use; ASTM-D790
 5.90 GPa
@Temperature -40.0 °C
856 ksi
@Temperature -40.0 °F
Absolute Drying; ASTM-D790
Izod Impact, Notched  0.600 J/cm
@Temperature -40.0 °C
1.12 ft-lb/in
@Temperature -40.0 °F
Absolute Drying; ASTM-D256
 0.820 J/cm
@Temperature -40.0 °C
1.54 ft-lb/in
@Temperature -40.0 °F
Practical Use; ASTM-D256
 1.05 J/cm
@Temperature 23.0 °C
1.97 ft-lb/in
@Temperature 73.4 °F
Absolute Drying; ASTM-D256
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Practical Use; ASTM-D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+9 ohm-cm1.00e+9 ohm-cmPractical Use; ASTM-D257
 1.00e+12 ohm-cm1.00e+12 ohm-cmAbsolute Drying; ASTM-D257
Dielectric Strength  16.0 kV/mm
@Thickness 2.00 mm
406 kV/in
@Thickness 0.0787 in
2mmt, Practical Use; ASTM-D149
 21.0 kV/mm
@Thickness 2.00 mm
533 kV/in
@Thickness 0.0787 in
Absolute Drying; ASTM-D149
Arc Resistance 120 sec120 secPractical Use; ASTM-D495
 130 sec130 secAbsolute Drying; ASTM-D495
Comparative Tracking Index >= 600 V>= 600 VIEC Method
 
Thermal PropertiesMetricEnglishComments
CTE, linear 74.0 µm/m-°C41.1 µin/in-°FAbsolute Drying; ASTM-D696
Deflection Temperature at 0.46 MPa (66 psi) 183 °C361 °FAbsolute Drying; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 96.0 °C205 °FAbsolute Drying; ASTM-D648
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Melt Temperature 260 - 280 °C500 - 536 °F
Mold Temperature 70.0 - 110 °C158 - 230 °F
Injection Pressure 50.0 - 60.0 MPa7250 - 8700 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® 8350 HS BK-102 PA6 (Dry)
Kolon KOPA® KN173HI3R High Impact Nylon 6
Adell BD-10 Nylon 6, Ultra High Impact
Ravago Manufacturing Americas Hylon® N2000STHL Nylon 6 (DAM)
BASF Ultramid® B50L 01 PA6 (Conditioned)

PTOY924 / 107475

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.