MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ineos ABS Triax® 3050 ABS/Nylon Alloy, Injection Molding Grade (DAM)  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS)/Nylon Blend; Nylon (Polyamide PA)

Material Notes: Triax® 3050 resin is an ABS (Acrylonitrile Butadiene Styrene)/Nylon 6 alloy for injection molding. It is a semicrystalline thermoplastic with improved stability to light exposure, excellent processability, good chemical resistance, good fatigue performance, and excellent abrasion characteristics. Triax® 3050 resin exhibits a good balance of impact strength and flow properties. Typical applications include interior automotive applications.

Triax® is now a INEOS Styrolution trade name; this grade is discontinued. Information provided by the manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.06 g/cc1.06 g/ccASTM-D792
Density 1.05 g/cc0.0380 lb/in³ASTM-D792
Water Absorption 1.1 %
@Time 86400 sec
1.1 %
@Time 24.0 hour
ASTM-D570
Water Absorption at Saturation 4.3 %4.3 %ASTM-D570
Linear Mold Shrinkage 0.0090 cm/cm0.0090 in/inASTM-D955
Linear Mold Shrinkage, Transverse 0.010 cm/cm0.010 in/inASTM-D955
Melt Flow 6.0 g/10 min
@Load 5.00 kg,
Temperature 260 °C
6.0 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM-D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 105105ASTM-D785
Tensile Strength, Yield 43.4 MPa6300 psiASTM-D638
Elongation at Break >= 50 %>= 50 %ASTM-D638
Tensile Modulus 2.17 GPa315 ksiASTM-D638
Flexural Yield Strength 75.2 MPa10900 psiASTM-D790
Flexural Modulus 2.07 GPa300 ksiASTM-D790
Izod Impact, Notched  0.694 J/cm
@Thickness 6.35 mm,
Temperature -40.0 °C
1.30 ft-lb/in
@Thickness 0.250 in,
Temperature -40.0 °F
ASTM-D256
 0.801 J/cm
@Thickness 3.17 mm,
Temperature -40.0 °C
1.50 ft-lb/in
@Thickness 0.125 in,
Temperature -40.0 °F
ASTM-D256
 7.47 J/cm
@Thickness 6.35 mm,
Temperature 22.8 °C
14.0 ft-lb/in
@Thickness 0.250 in,
Temperature 73.0 °F
ASTM-D256
 8.01 J/cm
@Thickness 3.17 mm,
Temperature 22.8 °C
15.0 ft-lb/in
@Thickness 0.125 in,
Temperature 73.0 °F
ASTM-D256
Instrumented Impact Total Energy 47.5 J
@Temperature -40.0 °C
35.0 ft-lb
@Temperature -40.0 °F
0.100-in.; 0.5-in. dart; 1.6-in. clamp; 7.6 mph; ASTM-D3763
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 8.30e+15 ohm8.30e+15 ohmASTM-D257
Dielectric Constant 3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
Tinfoil Electrodes; ASTM-D150
Dielectric Strength 16.7 kV/mm
@Thickness 1.57 mm
425 kV/in
@Thickness 0.0620 in
Short time under oil; ASTM-D149
Dissipation Factor 0.024
@Frequency 1e+6 Hz
0.024
@Frequency 1e+6 Hz
Tinfoil Electrodes; ASTM-D150
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi)  90.0 °C
@Thickness 3.17 mm
194 °F
@Thickness 0.125 in
Unannealed; ASTM-D648
 97.2 °C
@Thickness 6.35 mm
207 °F
@Thickness 0.250 in
Unannealed; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi)  65.0 °C
@Thickness 3.17 mm
149 °F
@Thickness 0.125 in
Unannealed; ASTM-D648
 73.9 °C
@Thickness 6.35 mm
165 °F
@Thickness 0.250 in
Unannealed; ASTM-D648
Vicat Softening Point 185 °C
@Load 1.00 kg
365 °F
@Load 2.20 lb
Rate B, 120°C/hour; ASTM-D1525
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 232 - 266 °C450 - 511 °FInjection Molding
Middle Barrel Temperature 232 - 266 °C450 - 511 °FInjection Molding
Front Barrel Temperature 232 - 266 °C450 - 511 °FInjection Molding
Nozzle Temperature 249 - 260 °C480 - 500 °FInjection Molding
Melt Temperature 238 - 271 °C460 - 520 °FInjection Molding
Mold Temperature 38.0 - 66.0 °C100 - 151 °FInjection Molding
Drying Temperature 88.0 °C
@Time 7200 - 14400 sec
190 °F
@Time 2.00 - 4.00 hour
Moisture Content 0.15 - 0.35 %0.15 - 0.35 %
Dew Point <= -29.0 °C<= -20.2 °Finlet air
Injection Pressure 41.4 - 82.7 MPa6000 - 12000 psiInjection Molding
Back Pressure 0.345 - 0.689 MPa50.0 - 100 psiInjection Molding
Clamp Pressure 46.2 - 77.0 MPa6700 - 11200 psiInjection Molding
Cushion <= 0.317 cm<= 0.125 inInjection Molding
 
Descriptive Properties
Hold Pressure30-50% of Injection Pressure, Injection Molding
Injection SpeedFastInjection Molding
Screw Compression Ratio2.5:1Injection Molding
Screw Length-to-Diameter Ratio>= 20:1Injection Molding
Screw SpeedModerate, Injection Molding
Shot Weight-to-Machine Capacity Ratio0.5-0.7Injection Molding

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Daicel CEVIAN® A1700 PA/ABS Alloy, DAM
Techmer ES Plastiblend® ABS/PA 1700
E-Polymers TEKAMID® H12TW Unreinforced Low warpage PA/ABS Alloy
INEOS Styrolution Triax® 1185 ABS/Nylon Alloy, Injection Molding Grade
Americhem Engineered Compounds ColorFast® NYA1000 Nylon/ABS Alloy

PINEA937 / 107208

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.