MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Type 254 SMO High-Nitrogen Austenitic Stainless Steel, Annealed Bar, Shapes, UNS S31254
Categories: Metal; Ferrous Metal; Stainless Steel; T S30000 Series Stainless Steel

Material Notes:

Information provided by MetalTek, Outokumpo, Industeel, Sandvik. and the references(s).

Key Words: ASTM A 276
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.00 g/ccRT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 650 MPa
Tensile Strength, Yield 300 MPa
Elongation at Break 35 %
Reduction of Area 50 %
Modulus of Elasticity 195 GPaRT
 166 GPa
@Temperature 400 °C
Poissons Ratio 0.30RT
Shear Modulus 75.0 GPacalculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000850 ohm-cmRT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.5 µm/m-°C
@Temperature 100 °C
 18.0 µm/m-°C
@Temperature 400 °C
Specific Heat Capacity 0.500 J/g-°CRT
Thermal Conductivity 14.0 W/m-KRT
 18.0 W/m-K
@Temperature 400 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.025 %
Chromium, Cr 19.5 - 20.5 %
Copper, Cu 0.50 - 1.0 %
Iron, Fe 49.535 - 56.32 %As Balance
Manganese, Mn <= 1.2 %
Molybdenum, Mo 6.0 - 7.0 %
Nickel, Ni 17.5 - 19.5 %
Nitrogen, N 0.18 - 0.24 %
Silicon, Si <= 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Type 254 SMO High-Nitrogen Austenitic Stainless Steel, Annealed Plate, Sheet, Strip, UNS S31254
MetalTek 254 SMO® Super Austenitic Stainless Steel
309 Stainless Steel, annealed, sheet
316 Stainless Steel, annealed bar
Oxygen-free Copper (OF), UNS C10200, H55 (15%) temper, tubing

MQZ9917 / 172151

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.