MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Azoty Tarnow™ TARNOFORM 411 POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Unreinforced

Material Notes: Easy flowing, internally strengthened grade for injection molding of thin walled parts of very high mechanical requirements.

Information provided by Zakłady Azotowe w Tarnowie-Moscicach S.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³ISO 1183
Linear Mold Shrinkage 0.036 cm/cm0.036 in/in60x60x4
Linear Mold Shrinkage, Transverse 0.0335 cm/cm0.0335 in/inISO 294-4
Melt Flow 13 g/10 min
@Load 2.16 kg,
Temperature 190 °C
13 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 118118ISO 2039-2
Ball Indentation Hardness 155 MPa22500 psi358 N; ISO 2039-1
Tensile Strength, Yield 68.0 MPa9860 psiISO 527
Elongation at Break 30 %30 %ISO 527
Flexural Strength 68.0 MPa9860 psiISO 178
Izod Impact, Notched (ISO) 6.00 kJ/m²2.86 ft-lb/in²1A; ISO 180
Charpy Impact, Notched 0.600 J/cm²2.86 ft-lb/in²1eA; ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 60093
Dielectric Constant 3.9
@Frequency 1e+6 Hz
3.9
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 25.0 kV/mm635 kV/inIEC 60243
Dissipation Factor 0.0085
@Frequency 1e+6 Hz
0.0085
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 1.9 sec1.9 sec
Comparative Tracking Index 600 V600 VIEC 112
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 1.48 J/g-°C0.354 BTU/lb-°F
Melting Point 170 °C338 °F10°C/min.; ISO 3146
Maximum Service Temperature, Air 100 °C212 °F
Deflection Temperature at 1.8 MPa (264 psi) 115 °C239 °FISO 75
Vicat Softening Point 161 °C322 °F50 N; ISO 306
Flammability, UL94 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 - 230 °C356 - 446 °FBarrel temperature
Mold Temperature 60.0 - 120 °C140 - 248 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Bayblend® FR3040 PC/ABS Blend
Celanese Zytel® 73G30HSL BK416 PA6-GF30
Azoty Tarnow™ Tarnamid® T-27 GF30 I Polyamide 6 - Glass Fiber Reinforced

PZAK032 / 72871

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.