MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ATI Allegheny Ludlum AL 4565™ Corrosion Resistant Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel; T S30000 Series Stainless Steel

Material Notes: Characteristics:
  • Very high resistance to pitting and crevice corrosion
  • Excellent general corrosion resistance in a variety of media
  • Higher mechanical propertied then conventional stainless steels
  • Good weldability and metallurgical stability
  • Good resistance to stress corrosion cracking
  • Information provided by Allegheny Ludlum

    Key Words: UNS S34565, EN 1.4565
    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 8.00 g/cc0.289 lb/in³
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Rockwell B 9090
    Tensile Strength, Ultimate 903 MPa131000 psi
     630 MPa
    @Temperature 300 °C
    91400 psi
    @Temperature 572 °F
     725 MPa
    @Temperature 100 °C
    105000 psi
    @Temperature 212 °F
    Tensile Strength, Yield  240 MPa
    @Temperature 300 °C
    34800 psi
    @Temperature 572 °F
     345 MPa
    @Temperature 100 °C
    50000 psi
    @Temperature 212 °F
     469 MPa
    @Strain 0.2 %
    68000 psi
    @Strain 0.2 %
    Elongation at Break 47 %47 %
     45 %
    @Temperature 100 °C
    45 %
    @Temperature 212 °F
     45 %
    @Temperature 300 °C
    45 %
    @Temperature 572 °F
    Modulus of Elasticity 195 GPa28300 ksi
     
    Electrical PropertiesMetricEnglishComments
    Volume Resistivity 0.000092 ohm-cm0.000092 ohm-cm
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear  15.0 µm/m-°C
    @Temperature 20.0 - 100 °C
    8.33 µin/in-°F
    @Temperature 68.0 - 212 °F
     17.3 µm/m-°C
    @Temperature 20.0 - 500 °C
    9.61 µin/in-°F
    @Temperature 68.0 - 932 °F
    Specific Heat Capacity  0.450 J/g-°C
    @Temperature 20.0 - 100 °C
    0.108 BTU/lb-°F
    @Temperature 68.0 - 212 °F
     0.550 J/g-°C
    @Temperature 20.0 - 300 °C
    0.131 BTU/lb-°F
    @Temperature 68.0 - 572 °F
     0.620 J/g-°C
    @Temperature 20.0 - 500 °C
    0.148 BTU/lb-°F
    @Temperature 68.0 - 932 °F
    Thermal Conductivity  13.0 W/m-K
    @Temperature 20.0 - 100 °C
    90.2 BTU-in/hr-ft²-°F
    @Temperature 68.0 - 212 °F
     15.0 W/m-K
    @Temperature 20.0 - 500 °C
    104 BTU-in/hr-ft²-°F
    @Temperature 68.0 - 932 °F
     
    Component Elements PropertiesMetricEnglishComments
    Carbon, C 0.010 %0.010 %
    Chromium, Cr 24 %24 %
    Iron, Fe >= 48.04 %>= 48.04 %As Remainder
    Manganese, Mn 6.0 %6.0 %
    Molybdenum, Mo 4.5 %4.5 %
    Nickel, Ni 17 %17 %
    Nitrogen, N 0.45 %0.45 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    ASTM A500 Steel, grade A, Round Structural Tubing
    ATI Allegheny Ludlum AL 453™ Stainless Steel
    Cotronics Resbond™ 954 High Temperature Ceramic Adhesive, Stainless Steel Composition
    Morgan Advanced Ceramics Kao-Lok® Hardware for Blanket Wallpaper Systems 304SS Washers and Studs
    2519 Aluminum Composition Spec

    NL1022 / 17790

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.