MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

CENTROPLAST CENTROCARB GF Polycarbonate 30% glass fiber
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, 30% Glass Filled

Material Notes: CENTROCARB GF is a transparent or semi-transparent plastic, reinforced for high strength and impact resistance. It has a high tensile modulus of elasticity and is well suited for structural elements, and insulating components.

Information provided by CENTROPLAST Engineering Plastics GMBH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.43 g/cc0.0517 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.080 %0.080 %in normal climate 23°C/50%RH; ISO 62
Water Absorption at Saturation 0.20 %0.20 %in water at 23°C; ISO 62
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 150 MPa21800 psivalue at 30 sec.; ISO 2039-1
Tensile Strength at Break 55.0 MPa7980 psiv = 5 mm/min; ISO 527-2
Elongation at Break 4.0 %4.0 %ISO 527-2
Tensile Modulus 5.00 GPa725 ksiISO 527-2
Flexural Modulus 4.70 GPa682 ksiISO 178
Charpy Impact Unnotched 4.50 J/cm²21.4 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 0.800 J/cm²3.81 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmIEC 60093
Surface Resistance 1.00e+16 ohm1.00e+16 ohmIEC 60093
Dielectric Constant  3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
 3.6
@Frequency 100 Hz
3.6
@Frequency 100 Hz
IEC 60250
Dielectric Strength 36.0 kV/mm914 kV/inin transformer oil; IEC 60243-1
Dissipation Factor  0.0010
@Frequency 100 Hz
0.0010
@Frequency 100 Hz
IEC 60250
 0.0080
@Frequency 1e+6 Hz
0.0080
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 175 V175 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 40.0 µm/m-°C
@Temperature 20.0 °C
22.2 µin/in-°F
@Temperature 68.0 °F
ISO 11359
Thermal Conductivity 0.240 W/m-K1.67 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 120 °C248 °FLong Term
 140 °C284 °FShort term
Deflection Temperature at 1.8 MPa (264 psi) 135 °C275 °FISO 75-2
Vicat Softening Point 148 °C298 °FVST/B/50; ISO 306
Flammability, UL94  V-2
@Thickness 3.00 mm
V-2
@Thickness 0.118 in
 V-2
@Thickness 6.00 mm
V-2
@Thickness 0.236 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 46, Unreinforced
Overview of materials for PVC, High Impact
Westlake Plastics Zelux® 30% GF Polycarbonate
Covestro Bayblend® KU 2-1480 Polycarbonate/ABS Blend
Overview of materials for Polypropylene, Extrusion Grade

PCENTR36 / 27987

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.