MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

DuPont Mobility and Materials Delrin® 1260 NC010 Acetal Copoly  (discontinued **)
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Features:
  • Colorable
  • Dimensional Stability, Good
  • Viscosity, Low
  • Printable
  • Spin Weldable
  • Ultrasonic Weldable
  • Vibration Weldable
Uses:
  • Parts, Engineering
  • Gears
  • Fasteners

Information provided by DuPont; The Delrin product line was sold by DuPont in 2023 but this specific grade was discontinued prior to the sale

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³ISO 1183
Water Absorption 0.28 %0.28 %Immersion 24h; Similar to ISO 62
 0.35 %0.35 %Immersion 24h; Similar to ISO 62
Water Absorption at Saturation 0.70 %0.70 %Similar to ISO 62
Linear Mold Shrinkage, Flow 0.019 cm/cm0.019 in/in2.0 mm; ISO 294-4
Linear Mold Shrinkage, Transverse 0.018 cm/cm0.018 in/in2.0 mm; ISO 294-4
Melt Flow 25 g/10 min25 g/10 mincm³/10 min; 190°C/2.16 kg; ISO 1133
 29 g/10 min29 g/10 minISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8686ISO 2039/2
Hardness, Rockwell R 118118ISO 2039/2
Tensile Strength, Yield 64.0 MPa9280 psiISO 527
Elongation at Break 20 %20 %Nominal; ISO 527
Elongation at Yield 7.0 %7.0 %ISO 527
Tensile Modulus 2.90 GPa421 ksiISO 527
Flexural Yield Strength 76.0 MPa11000 psiFlexural Stress at 3.5% Strain; ISO 178
Flexural Modulus 2.70 GPa392 ksiISO 178
Izod Impact, Notched (ISO) 6.00 kJ/m²2.86 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched 16.0 J/cm²76.1 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 0.600 J/cm²2.86 ft-lb/in²ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 9.00e+12 ohm-cm9.00e+12 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.83.8100 Hz; IEC 60250
 3.83.81 MHz; IEC 60250
Dissipation Factor 0.00140.0014100 Hz; IEC 60250
 0.00430.00431 MHz; IEC 60250
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C
@Temperature 23.0 - 55.0 °C
61.1 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
66.7 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1/-2
Melting Point 168 °C334 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 157 °C315 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °C203 °FISO 75-1/-2
UL RTI, Electrical 105 °C221 °F3.0 mm; UL 746B
 105 °C221 °F1.5 mm; UL 746B
 105 °C221 °F0.75 mm; UL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °F1.5 mm; UL 746B
 80.0 °C176 °F0.75 mm; UL 746B
 85.0 °C185 °F3.0 mm; UL 746B
UL RTI, Mechanical without Impact 90.0 °C194 °F3.0 mm; UL 746B
 90.0 °C194 °F1.5 mm; UL 746B
 90.0 °C194 °F0.75 mm; UL 746B
Flammability, UL94 HBHB3.0 mm; UL94
 HBHB3.0 mm; IEC 60695-11-10
 HBHB1.5 mm; IEC 60695-11-10
 HBHB1.5 mm; UL94
 HBHB0.75 mm; IEC 60695-11-10
 HBHB0.75 mm; UL94
 
Processing PropertiesMetricEnglishComments
Melt Temperature 190 - 210 °C374 - 410 °F
Mold Temperature 80.0 - 100 °C176 - 212 °F
Moisture Content <= 0.20 %<= 0.20 %
 
Descriptive Properties
ColorNatural
FormPellets
Processing MethodInjection Moldable
 Injection Molding
Region AvailableAmericas
 Asia/Pacific
 Europe

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDTA9076 / 32051

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.