MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Master Bond Supreme 42HT-2ND Black Two component, non-flow epoxy system
Categories: Polymer; Thermoset; Epoxy

Material Notes: Key Features:
  • Convenient processing
  • Superior thermal cycling capabilities
  • Meets NASA low outgassing specifications
  • Withstands 1,000 hours 85°C/85% RH
Product Description: Master Bond Supreme 42HT-2ND Black is a special two part epoxy system combining robust temperature and chemical resistance, very good toughness and a smooth, non-flowing viscosity. Supreme 42HT-2ND Black is easy to use with a forgiving mix ratio of 100 to 40 by weight or 100 to 50 by volume. Supreme 42HT-2ND Black is a lower exotherm type system with a longer working life. It cures in 48-72 hours at ambient temperatures and in 2-3 hours at 200°F. The optimum cure schedule is overnight at room temperature followed by 3-5 hours at 160-200°F. The system is 100% reactive with no solvents or diluents, which imparts low shrinkage upon curing. This epoxy bonds well to a wide variety of substrates including metals, composites, ceramics, glass and many plastics. Its toughness allows it to be well suited for bonding dissimilar substrates and to withstand rigorous thermal cycling. Additionally, the cured epoxy is a superb electrical insulator. It resists a wide range of chemicals including many acids, bases, solvents, fuels and oils. Its service temperature range is 4K to +450°F. The color of Part A is black and Part B is amber. This versatile system can be used in aerospace, electronic, optical and OEM industries, particularly when vacuum compatibility along with the other product properties mentioned previously are desirable.

Product Advantages:

  • Non-critical mix ratio: 100 to 40 by weight and 100 to 50 by volume
  • Lower exotherm system, longer working life
  • Outstanding temperature and chemical resistance
  • Reliable electrical insulator
  • Gun dispensable
  • Cryogenically serviceable

Information provided by Master Bond.

Vendors: Master Bond is a leading manufacturer of adhesives, sealants, coatings and potting compounds. Master Bond’s vast product line consists of over 3,000 epoxy, polyurethane, silicone, cyanoacrylate and latex adhesives that vary in viscosity, cure speed, strength, chemical resistance, electrical properties, etc. Our custom adhesives offer design flexibility and provide excellent bonding performance. Visit www.masterbond.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 75 - 8575 - 85
 8585after 1,000 hours 85°C/85% RH
Tensile Strength 62.1 - 68.9 MPa9000 - 10000 psi
Tensile Modulus 2.07 - 2.41 GPa300 - 350 ksi
Adhesive Bond Strength 12.4 - 13.8 MPa1800 - 2000 psiTensile lap shear, Al to Al
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cm
Dielectric Constant 4.5
@Frequency 60 Hz
4.5
@Frequency 60 Hz
Dielectric Strength 17.3 kV/mm
@Thickness 3.17 mm
440 kV/in
@Thickness 0.125 in
 
Thermal PropertiesMetricEnglishComments
CTE, linear 45.0 - 50.0 µm/m-°C25.0 - 27.8 µin/in-°F
Maximum Service Temperature, Air 232 °C450 °F
Minimum Service Temperature, Air -269 °C-452 °F
Glass Transition Temp, Tg 130 - 135 °C266 - 275 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  120 - 180 min
@Temperature 93.3 °C
2.00 - 3.00 hour
@Temperature 200 °F
Option 2
 180 - 300 min
@Temperature 71.1 - 93.3 °C
3.00 - 5.00 hour
@Temperature 160 - 200 °F
Optimum: overnight at 75°F followed by 3-5 hours at 160-200°F
 2880 - 4320 min
@Temperature 23.9 °C
48.0 - 72.0 hour
@Temperature 75.0 °F
Option 1
Working Life 60.0 - 90.0 min60.0 - 90.0 minafter mixing, 100 gram batch
Shelf Life 1.00 Month1.00 Monthin cans, in original, unopened containers
 6.00 Month6.00 Monthin syringes, in original, unopened containers
 
Descriptive Properties
Mixing ratio100:40 by weightParts A to B
 100:50 by volumeParts A to B
ViscositypastePart A
 pastePart B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PMASTM5941 / 306830

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.