MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC NORYL PPX™ Resin PPX7115F Polyphenylene Ether + PP (PPE+PP)
Categories: Polymer; Thermoplastic; Polyphenylene Ether/PPO; Polypropylene (PP)

Material Notes: NORYL PPX™ 7115F resin is a non-reinforced alloy of polyphenylene ether (PPE) + polypropylene (PP). This FDA certified injection moldable grade exhibits high impact resistance and good heat resistance along with hydrolytic and dimensional stability. NORYL PPX7115F resin is an excellent candidate for food contact applications requiring high impact, chemical resistance, and good heat performance.

Features: Hydrolytic Stability,Chemical Resistance,Low Creep Sensitivity,Low Warpage,High Impact Resistance,Food Contact Acceptable

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.990 g/cc0.990 g/ccASTM D792
Moisture Absorption 0.0200 %0.0200 %Injection Molding
Viscosity 12 cP
@Load 5.00 kg,
Temperature 260 °C
12 cP
@Load 11.0 lb,
Temperature 500 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0060 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0060 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse 0.0060 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0060 - 0.0080 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 14 g/10 min
@Load 5.00 kg,
Temperature 260 °C
14 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 34.0 MPa4930 psi50 mm/min; ASTM D638
Tensile Strength, Yield 35.0 MPa5080 psi50 mm/min; ASTM D638
 35.0 MPa5080 psi50 mm/min; ISO 527
Elongation at Break 75 %75 %50 mm/min; ISO 527
 125 %125 %50 mm/min; ASTM D638
Elongation at Yield 8.0 %8.0 %50 mm/min; ASTM D638
Tensile Modulus 1.24 GPa180 ksi50 mm/min; ASTM D638
 1.37 GPa199 ksi1 mm/min; ISO 527
Flexural Strength 51.0 MPa7400 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 1.37 GPa199 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 534 J394 ft-lbASTM D256
Dart Drop, Total Energy 37.0 J27.3 ft-lbASTM D3763
 30.0 J
@Temperature -30.0 °C
22.1 ft-lb
@Temperature -22.0 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 162 µm/m-°C
@Temperature -40.0 - 40.0 °C
90.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow 97.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
54.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 112 °C
@Thickness 3.20 mm
234 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C
@Thickness 3.20 mm
185 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 86.0 °C187 °FRate B/50; ASTM D1525
 131 °C268 °FRate A/50; ISO 306
Flammability, UL94 HB
@Thickness >=1.50 mm
HB
@Thickness >=0.0591 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 260 - 290 °C500 - 554 °F
Zone 2 240 - 280 °C464 - 536 °F
Zone 3 250 - 290 °C482 - 554 °F
Melt Temperature 260 - 290 °C500 - 554 °FInjection Molding
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F
Drying Temperature 60.0 - 65.0 °C140 - 149 °FInjection Molding
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection Molding
 8.00 hour8.00 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 30 - 70 %30 - 70 %
Vent Depth 0.00380 - 0.00510 cm0.00150 - 0.00201 in
Screw Speed 20 - 100 rpm20 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82225 / 290172

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.