MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Refractory Metals

(Viewing data as-entered. Click here to return)
Schwarzkopf Plansee PM 2000, Bar Grain Class 6 ODS Iron Alloy Bar  (discontinued **)
Categories: Metal; Ferrous Metal; Metal Matrix Composite

Material Notes: The PLANSEE sophisticated PM 2000 is a highly oxidation resistant and extremely creep resistant ferritic iron-chromium based alloy. Homogeneous dispersion strengthening with nano sized Y2O3 particles in combination with recrystallized coarse grained microstructure gives PM 2000 highest hot strength and creep strength up to 1350°C. Due to its high content of Aluminium and Chromium, PM2000 forms a dense and adherent Al2O3 scale when used at high temperatures under oxidizing atmospheres. This oxide scale is highly resistant to high-speed gas flows up to 1300°C.

Advantages of PM 2000:

  • creep resistance up to 1350 °C
  • high hot strength up to 1300°C
  • excellent oxidation and hot corrosion resistance
  • highly resistant against coking and carburization compared to NiCr alloys
  • due to its lower density, components made from PM 2000 are lighter than those made from Ni base materials
  • high stability against high-speed gas flows at temperatures up to 1300 °C
  • good machinability with normal tooling
Typical fields of application for PM 2000:
  • thermocouple sleeves for high temperatures
  • burner nozzles
  • charge carriers for parts for high temperature furnace construction
  • pull rod assemblies for high temperature testing
  • stirrers for the glass industry
  • honey comb structures for aerospace
  • components for the chemical plant construction
  • combustion parts for engines

Key Words: Material No. 1.4768; Abbreviated DIN Name CrAl 21 6
Vendors: PLANSEE SE: Whether it's high temperatures, aggressive chemicals or extreme mechanical loading: PLANSEE supplies a suitable product solution in refractory metals or composite materials. As the world market leader in powder metallurgically produced high performance materials we combine outstanding materials knowledge with profound applications and technology know-how. Visit us at www.plansee.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.18 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 290HV 10
Tensile Strength, Ultimate 720 MPaBar
 65.0 MPa
@Temperature 1200 °C
 90.0 MPa
@Temperature 1000 °C
 96.0 MPa
@Temperature 900 °C
 122 MPa
@Temperature 800 °C
 210 MPa
@Temperature 700 °C
 340 MPa
@Temperature 600 °C
Tensile Strength, Yield 603 MPa
@Strain 0.2 %
 85.0 MPa
@Strain 0.2 %,
Temperature 1000 °C
 90.0 MPa
@Strain 0.2 %,
Temperature 900 °C
 120 MPa
@Strain 0.2 %,
Temperature 800 °C
 202 MPa
@Strain 0.2 %,
Temperature 700 °C
 328 MPa
@Strain 0.2 %,
Temperature 600 °C
Elongation at Break 14 %
 14 %
@Temperature 1000 °C
A5
 26 %
@Temperature 900 °C
A5
 33 %
@Temperature 600 °C
A5
 36 %
@Temperature 800 °C
A5
 38 %
@Temperature 700 °C
A5
Modulus of Elasticity 140 GPa
@Temperature 950 °C
 155 GPa
@Temperature 800 °C
 160 GPa
@Temperature 700 °C
 172 GPa
@Temperature 600 °C
 185 GPa
@Temperature 400 °C
 205 GPa
@Temperature 200 °C
 215 GPa
@Diameter 15.0 mm
bar
Fracture Toughness 34.0 MPa-m½
Impact 15J/cm²; Notched 9 mm Bar DVKM Sample
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000131 ohm-cm
Magnetic Coercive Force, Hc 3.64 Oe
Curie Temperature 553 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.7 µm/m-°C
@Temperature 20.0 °C
 12.0 µm/m-°C
@Temperature 100 °C
Longitudinal
 12.2 µm/m-°C
@Temperature 250 °C
Longitudinal
 12.5 µm/m-°C
@Temperature 500 °C
Longitudinal
 15.1 µm/m-°C
@Temperature 1000 °C
Longitudinal
CTE, linear, Transverse to Flow 11.5 µm/m-°C
@Temperature 100 °C
 11.6 µm/m-°C
@Temperature 250 °C
 12.0 µm/m-°C
@Temperature 500 °C
 14.5 µm/m-°C
@Temperature 100 °C
Specific Heat Capacity 0.480 J/g-°C
 0.480 J/g-°C
@Temperature 200 °C
 0.500 J/g-°C
@Temperature 100 °C
 0.610 J/g-°C
@Temperature 500 °C
 0.680 J/g-°C
@Temperature 750 °C
 0.740 J/g-°C
@Temperature 1000 °C
Thermal Conductivity 10.9 W/m-K
 16.0 W/m-K
@Temperature 200 °C
 21.0 W/m-K
@Temperature 500 °C
 22.0 W/m-K
@Temperature 750 °C
 25.5 W/m-K
@Temperature 1000 °C
 28.0 W/m-K
@Temperature 1200 °C
Melting Point 1483 °C
Maximum Service Temperature, Air 1350 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 5.5 %
Chromium, Cr 19 %
Iron, Fe 74.5 %As Remainder
Titanium, Ti 0.50 %
Y2O3 0.50 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Schwarzkopf Plansee PM 2000 Grain Class 4 ODS Iron Alloy
Schwarzkopf Plansee PM 2000, Sheet Grain Class 6 ODS Iron Alloy Sheet
AISI Type 316F Stainless Steel, annealed sheet
ATI Allegheny Ludlum Type 316 Stainless Steel, UNS S31600
COI Ceramics Sylramic™ Crystalline Silicon Carbide (SiC) Fiber

NPLAN10 / 18811

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.