MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Eastman 1830F Polyethylene  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE)

Material Notes: Polyethylene 1830F is a low-density formulation with no slip or antiblock. It is suggested for film applications requiring high clarity, good tear and impact strength, a wide heat sealing range and good printability. This product may be used as a component of packages used for holding food during cooking

List of Applications:

  • Converter film for food
  • Flexible medical
  • Industrial packaging

low density polyethylene 1830F may lawfully be used in food-contact applications under FDA regulations at 21 CFR 177.1520(c)(2.2).

Information supplied by the manufacturer.

Information from manufacturer data sheet.

Eastman Chemical Company sold its polyethylene business to Westlake Chemical Corporation in Dec. 2006. This grade no longer appears in the Westlake product line.

Key Words: High clarity, good tear and impact strength, a wide heat sealing range and good printability
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.920 g/ccASTM D4883
Moisture Vapor Transmission 18.6 cc-mm/m²-24hr-atmASTM F372
Oxygen Transmission 200 cc-mm/m²-24hr-atmASTM D1434
Thickness 38.0 microns
Melt Flow 1.7 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 34.0 MPaASTM D882
Film Tensile Strength at Yield, TD 11.0 MPaASTM D882
Film Elongation at Break, MD 300 %ASTM D882
Film Elongation at Break, TD 850 %ASTM D882
Secant Modulus, MD 0.207 GPa1% Secant; ASTM D882
Secant Modulus, TD 0.240 GPa1% Secant; ASTM D882
Coefficient of Friction >= 2.0ASTM D1894
Elmendorf Tear Strength MD 500 g
Elmendorf Tear Strength TD 130 g
Elmendorf Tear Strength, MD 13.2 g/micronASTM D1922
Elmendorf Tear Strength, TD 3.40 g/micronASTM D1922
Dart Drop 2.90 g/micronASTM D1709A
Film Tensile Strength at Break, MD 34.0 MPaASTM D882
Film Tensile Strength at Break, TD 23.0 MPaASTM D882
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 95.0 °CASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 6.0 %ASTM D1003
Gloss 70 %at 45°; ASTM D2457
Transmission, Visible 95 %ASTM D1746
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.
 
Descriptive Properties
ProcessFilm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eastman 1830A Polyethylene
Eastman 1830E Polyethylene
Eastman Tenite Polyethylene 1810A Low Density Polyethylene - Molding
Changzhou Jinlibao GETAILONG JLB-110800 APET Sheet
Corning Willow® Flexible Display Glass

PEAT255 / 35360

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.