MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Röchling GLASTHERM HT220 Insulation Sheet
Categories: Polymer; Thermoset; Composite SMC; Filled/Reinforced Thermoset; Polyester, TS

Material Notes: Glastherm Grade HT220 is a thermal insulation sheet that is a highly heat-resistant material that combines low thermal conductivity with very high compressive strength at molding temperature. It is ideal for many of the more difficult molding applications.

Information provided by Glastic Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.85 g/ccASTM D-792
Water Absorption 0.20 %% by wt.; ASTM D-570
 
Mechanical PropertiesOriginal ValueComments
Flexural Strength 52200 psiASTM D-790
Compressive Strength 35000 psi
@Temperature 288 °C
ASTM D-695
 40600 psi
@Temperature 200 °C
ASTM D-695
 55100 psi
@Temperature 150 °C
ASTM D-695
 72500 psi
@Temperature 20.0 °C
ASTM D-695
Compressive Modulus 2.61e+6 psiASTM D-695
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.0 µm/m-°C
@Temperature 20.0 °C
Across Surface; ASTM D-696
 57.0 µm/m-°C
@Temperature 20.0 °C
Across Thickness; ASTM D-696
Thermal Conductivity 0.250 W/m-KASTM C-177
Maximum Service Temperature, Air 450 °F
 608 °F
 
Descriptive Properties
Standard ColorLight Beige
Thickness Tolerance in± 0.004

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Röchling Glastic BMC 1401 GTP Glass-Reinforced Polyester
Menzolit Menzolit® SMC 0180 Unsaturated Polyester UP
A. Schulman Premi-Glas® 2206-15 CR-SX Fiberglass Reinforced Thermoset SMC
Owens Corning Glass Fiber Reinforced Polyester SMC (Compression), 22 wt.% glass
Röchling GLASTHERM HT250 Insulation Sheet

PGLASW7 / 41941

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.