MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LG Chemical TR-558 Transparent ABS, Humidity Resistance, Natural and Colored Pellets  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Transparent, Molded

Material Notes: LG transparent ABS has excellent transparency, impact strength, stiffness, and processability. Since its properties are well balanced, it can be applied widely to a variety of electric and electronic parts, OA machines, toys and others that require transparency and high impact strength. An Izod impact strength or falling dart impact strength of LG transparent ABS is relatively similar to that of general ABS, it is not easily cracked like SAN or PMMA resin in the condition of low impact energy. TR-558 series is good for applications requiring high stiffness.

Information Provided by LG Chem

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.08 g/ccASTM D792
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cmASTM D955
Melt Index of Compound 20 g/10 minASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 112ASTM D785
Tensile Strength at Break 47.86 MPaASTM D638
Elongation at Break 50 %ASTM D638
Flexural Strength 78.45 MPaASTM D790
Flexural Modulus 2.34 GPaASTM D790
Izod Impact, Notched 9.81 J/mASTM D256
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 90.0 °CHeat deflection temperature, load unknown; ASTM D648
Flammability, UL94 HB
 
Optical PropertiesOriginal ValueComments
Haze 3.1 %
Transmission, Visible 90 %
 
Processing PropertiesOriginal ValueComments
Processing Temperature 190 - 200 °CExtrusion cylinder temperature, C1
 210 - 225 °CExtrusion cylinder temperature, C2
 230 - 240 °CExtrusion cylinder temperature, C3
 240 - 250 °CExtrusion cylinder temperature, C4 and C5
Rear Barrel Temperature 190 - 200 °C
Middle Barrel Temperature 200 - 220 °C
Front Barrel Temperature 210 - 230 °C
Nozzle Temperature 210 - 230 °C
Adapter Temperature 235 - 245 °C
Die Temperature 235 - 245 °F
Melt Temperature 220 - 240 °CInjection molding
 255 - 260 °CExtrusion
Mold Temperature 40.0 - 60.0 °C
Roll Temperature 75.0 - 85.0 °CBottom
 80.0 - 90.0 °CMiddle
 85.0 - 95.0 °CTop
Injection Pressure 68.65 - 88.26 MPaSecond
 58.84 - 98.1 MPaFirst
Back Pressure 0.490 - 1.96 MPa
Screw Speed 50 - 100 rpm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Versalis Sinkral® PD L 322 ABS Resin
LG Chemical AT-553 Transparent ABS, Permanent Antistatic, Natural and Colored Pellets
INEOS Styrolution Novodur® BX13036 ABS + PMMA
LG Chemical TR-558A ABS, Transparent, High Strength
LG Chemical TR-558AI Transparent ABS, High Stiffness, Ice Colored Pellets

PLGCHEM180 / 51001

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.